Photocuring 3D printing ceramic slurry as well as preparation method and application thereof

By optimizing the particle size grading and dispersant of ceramic powder, the problems of high viscosity and low solid content of ceramic slurry are solved, and low viscosity and high solid content of ceramic slurry are prepared, achieving high precision, high efficiency forming and complex structure The production of ceramic parts improves the mechanical properties and efficiency of ceramic parts.

CN118908725APending Publication Date: 2024-11-08ENLIGHTEN BEIJING IND TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410967278.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing ceramic photocuring 3D printing technology, the ceramic slurry has high viscosity and low solid content, resulting in poor forming accuracy, low structural density, low printing efficiency, and difficulty in removing slurry from internal pores, affecting the ceramic parts. Mechanical properties and surface quality.

Method used

By optimizing the particle size grading of ceramic powder and combining the use of dispersants and photoinitiators, low viscosity and high solid content ceramic slurry is prepared. The method of adding dispersants in step by step is used to optimize the flowability and forming of ceramic slurry. performance.

Benefits of technology

It realizes high-precision and efficient forming ceramic parts, improves the mechanical properties and durability of ceramic parts, and successfully prepares ceramic parts with complex microporous structures, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908725A_ABST
    Figure CN118908725A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of 3D printing materials, and discloses photocuring 3D printing ceramic slurry as well as a preparation method and application thereof. The ceramic slurry comprises ceramic powder; wherein the ceramic powder comprises the following components in percentage by mass: 5-25% of ceramic powder with the average particle size of 4 mu m, 10-40% of ceramic powder with the average particle size of 1 mu m and 40-80% of ceramic powder with the average particle size of 0.2 mu m. Mixing a part of the dispersing agent with the ceramic powder, and reacting to obtain modified ceramic powder; mixing the modified ceramic powder with an active diluent, an active monomer and a photoinitiator, and performing first ball milling to obtain primary ceramic slurry; and mixing the primary ceramic slurry with the residual dispersant, and carrying out second ball milling to obtain the ceramic slurry. The photocuring 3D printing ceramic slurry provided by the invention has the characteristics of low viscosity and high solid content, is good in fluidity, can efficiently form a high-precision ceramic part, and successfully prepares a ceramic part with a complex microporous structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of 3D printing materials, and in particular to a photocurable 3D printing ceramic slurry. Background Art

[0002] In recent years, ceramic 3D printing technology has made initial progress and has attracted the attention of more and more scientific and technological workers. Common ceramic 3D printing technologies include selective laser sintering, selective laser melting, laminated object manufacturing, inkjet printing, robocasting and stereolithography. Compared with other 3D printing technologies, ceramic robocasting 3D printing technology has the advantages of high molding accuracy, simple operation and fast printing speed. Therefore, it has attracted the attention and research of a large number of scholars and has gradually become the mainstream molding method of ceramic 3D printing.

[0003] The raw materials for photocuring 3D printing are usually resin-based ceramic slurries, which have high viscosity and are not easy to prepare ceramic slurries with high solid content, low viscosity and good fluidity. Currently, commercial ceramic slurries on the market generally have high viscosity and poor fluidity. In addition, it is not easy to remove bubbles generated during the preparation of high-viscosity ceramic slurries, and the slurry is not easy to self-level during printing. At the same time, high-viscosity ceramic slurries are not conducive to cleaning, and the slurry remaining in the pores inside complex structure ceramic parts is difficult to remove, resulting in serious pore blockage and failure to meet the design requirements of the parts.

[0004] If the solid content of the photocurable ceramic slurry is too low, it means that the amount of ceramic added to the slurry is insufficient, and the density of the formed green body is likely to be low after sintering, which affects the degree of densification during the subsequent sintering process, thereby affecting the mechanical properties and structural strength of the final ceramic parts. In addition, too low a solid content will reduce the forming accuracy during the printing process, affect the dimensional accuracy and surface quality of the ceramic parts, and further affect its finishing performance and use effect; it will also make it difficult to remove organic matter in the green body, and the green body will be easily deformed and cracked after degreasing.

[0005] The following advantages can be achieved by achieving high solid content and low viscosity ceramic slurry: (1) Improving forming accuracy and surface quality. The ceramic particles in high solid content ceramic slurry are more compact, reducing the scattering effect of light in the slurry, thereby improving printing accuracy. This enables more delicate structures and more accurate dimensions to be obtained when preparing complex shapes and high-precision parts. Low viscosity ceramic slurry is easier to spread evenly during the printing process, reducing the boundaries between layers, thereby improving the surface finish of the finished product. This is particularly important for application scenarios that require high-precision surfaces, such as aerospace, biomedicine and other fields. (2) Enhancing the density and mechanical properties of ceramic parts. Ceramic slurry with high solid content can form a denser ceramic structure after sintering, thereby improving the mechanical properties of ceramic products, such as compressive strength and flexural strength. This is of great significance for application scenarios that need to withstand high stress and high load. Low viscosity ceramic slurry helps to reduce the pores and defects generated during the printing and sintering process, and improves the density of ceramic products. The densified ceramic structure has better wear resistance, corrosion resistance and high temperature resistance. (3) Improving printing efficiency. Ceramic slurries with high solid content and low viscosity can solidify faster during the printing process, thereby improving printing efficiency. This means that more ceramic products can be produced faster and production costs can be reduced.

[0006] When the solid content in the slurry is low, the interaction between particles is weak, the slurry has good fluidity, and is manifested as a lower viscosity. As the solid content increases, the distance between particles decreases, and the chances of mutual collision and friction increase, resulting in increased flow resistance of the slurry and increased viscosity.

[0007] Therefore, in order to obtain a ceramic slurry with good flowability and forming properties, the relationship between solid content and viscosity needs to be carefully balanced. At present, there is an urgent need in the art to develop a ceramic slurry with low viscosity and high solid content. Summary of the invention

[0008] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a photocurable 3D printing ceramic slurry and a preparation method and application thereof.

[0009] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a photocurable 3D printing ceramic slurry, wherein the ceramic slurry includes ceramic powder; wherein the ceramic powder includes the following components by mass percentage: 5-25% of ceramic powder with an average particle size of 4 μm, 10-40% of ceramic powder with an average particle size of 1 μm, and 40-80% of ceramic powder with an average particle size of 0.2 μm.

[0010] The second aspect of the present invention provides a method for preparing the photocurable 3D printing ceramic slurry according to the first aspect, characterized in that the method comprises the following steps:

[0011] (1) mixing a portion of the dispersant with the ceramic powder and reacting the mixture to obtain a modified ceramic powder;

[0012] (2) mixing the modified ceramic powder obtained in step (1) with a reactive diluent, a reactive monomer and a photoinitiator, and then performing a first ball milling to obtain a primary ceramic slurry;

[0013] (3) The primary ceramic slurry obtained in step (2) is mixed with the remaining dispersant and then subjected to a second ball milling to obtain the ceramic slurry.

[0014] The third aspect of the present invention provides a photocurable 3D printing ceramic slurry obtained by the preparation method described in the second aspect.

[0015] The fourth aspect of the present invention provides a porous ceramic skeleton made from the photocurable 3D printing ceramic slurry described in the first aspect or the third aspect.

[0016] The fifth aspect of the present invention provides the use of the porous ceramic skeleton described in the fourth aspect in the preparation of ceramic catalyst carriers and bioceramic implants.

[0017] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0018] (1) The photocurable 3D printing ceramic slurry provided by the present invention has the characteristics of low viscosity and high solid content, good fluidity, and can efficiently form high-precision ceramic parts and successfully prepare ceramic parts with complex microporous structures.

[0019] (2) The ceramic parts prepared by the photocuring 3D printing ceramic slurry provided by the present invention have excellent mechanical properties and durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The zirconia ceramic product is prepared by using the zirconia ceramic slurry of Example 1 of the present invention.

[0021] Figure 2 The alumina filter component is prepared using the alumina ceramic slurry of Example 3 of the present invention.

[0022] Figure 3 The barium titanate ceramic transducer is prepared by using the barium titanate ceramic slurry of Example 4 of the present invention. DETAILED DESCRIPTION

[0023] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0024] A first aspect of the present invention provides a photocurable 3D printing ceramic slurry, wherein the ceramic slurry comprises ceramic powder;

[0025] The ceramic powder comprises the following components by mass percentage: 5-25% of ceramic powder with an average particle size of 4 μm, 10-40% of ceramic powder with an average particle size of 1 μm, and 40-80% of ceramic powder with an average particle size of 0.2 μm.

[0026] The present invention optimizes the particle size distribution of ceramic powder to obtain a ceramic slurry with low viscosity and high solid content. The ceramic slurry has excellent flowability and forming properties and can be used to prepare high-precision and high-performance ceramic parts.

[0027] In the present invention, the average particle size (D50) is measured by a Malvern laser particle size analyzer.

[0028] The mass percentage of the ceramic powder having an average particle size of 4 μm is, for example, 5%, 10%, 15%, 20%, 25%, and any value within the range of any two of the above values.

[0029] The mass percentage of the ceramic powder having an average particle size of 1 μm is, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, and any value within the range of any two of the above values.

[0030] The mass percentage of the ceramic powder with an average particle size of 0.2 μm is, for example, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, and any value within the range of any two of the above values.

[0031] In some embodiments of the present invention, the ceramic powder comprises the following components by mass percentage: 10-20% ceramic powder with an average particle size of 4 μm, 20-30% ceramic powder with an average particle size of 1 μm, and 50-70% ceramic powder with an average particle size of 0.2 μm.

[0032] In some embodiments of the present invention, the ceramic powder comprises the following components by mass percentage: 20% ceramic powder with an average particle size of 4 μm, 30% ceramic powder with an average particle size of 1 μm, and 50% ceramic powder with an average particle size of 0.2 μm.

[0033] In some embodiments of the present invention, the ceramic slurry further includes a photoinitiator, a reactive diluent, a reactive monomer and a dispersant.

[0034] In some embodiments of the present invention, the ceramic slurry comprises the following components by mass percentage: 70-80% ceramic powder, 0.1-1% photoinitiator, 5-15% active diluent, 10-20% active monomer and 1-6% dispersant.

[0035] In some embodiments of the present invention, the material of the ceramic powder is selected from at least one of silicon oxide, aluminum oxide, zirconium oxide, barium titanate, silicon carbide and silicon nitride.

[0036] In some embodiments of the present invention, the photoinitiator is selected from at least one of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator 819), bis(2,6-difluoro-3-pyrrolophenyl)titanium (photoinitiator 784), 2-hydroxy-2-methyl-1-phenyl-1-propanone (photoinitiator 1173), and a,a-dimethoxy-a-phenylacetophenone (photoinitiator 651).

[0037] In some embodiments of the present invention, the active diluent is selected from at least one of isobornyl acrylate (IBOA), acryloyl morpholine (ACMO), β-hydroxyethyl methacrylate (HEMA), 1,6-hexanediol diacrylate (HDDA), tridecyl acrylate (TDA), dodecyl methacrylate (LMA), lauryl acrylate (LA) and 1,6-hexanediol dimethacrylate (HDDMA).

[0038] In some embodiments of the present invention, the active monomer is selected from at least one of polyethylene glycol diacrylate (PEGDA), diethylene glycol diacrylate (DEGDA), ethoxylated trimethylolpropane triacrylate (TMPTA) and ethoxylated pentaerythritol tetraacrylate (PETA).

[0039] In some embodiments of the present invention, the dispersant is selected from at least one of polymer hyperdispersants, and the polymer hyperdispersant is selected from at least one of BYK-110, BYK-111, BYK-2205, BYK-163, BYK-199, KOS110, and KOS163.

[0040] The second aspect of the present invention provides a method for preparing the photocurable 3D printing ceramic slurry according to the first aspect, wherein the method comprises the following steps:

[0041] (1) mixing a portion of the dispersant with the ceramic powder and reacting the mixture to obtain a modified ceramic powder;

[0042] (2) mixing the modified ceramic powder obtained in step (1) with a reactive diluent, a reactive monomer and a photoinitiator, and then performing a first ball milling to obtain a primary ceramic slurry;

[0043] (3) The primary ceramic slurry obtained in step (2) is mixed with the remaining dispersant and then subjected to a second ball milling to obtain the ceramic slurry.

[0044] The preparation method of the present invention is simple and time-saving, and is conducive to the mass production of customized, complex and refined ceramic parts. The present invention adopts a method of adding dispersants in steps, which is more conducive to the preparation of low-viscosity, high-solid content ceramic slurry.

[0045] In some embodiments of the present invention, the mass ratio of the partial dispersant described in step (1) to the remaining dispersant described in step (3) is 0.3-13.5:2, preferably 1.8-3:2. In the present invention, all dispersants are added step by step according to a specific ratio to optimize the effect to the greatest extent.

[0046] In some embodiments of the present invention, the reaction time of step (1) is 1-5 hours.

[0047] In some embodiments of the present invention, the time of the first ball milling in step (2) is 0.5-2h.

[0048] In some embodiments of the present invention, the time of the second ball milling in step (3) is 0.5-1 h.

[0049] According to a particularly preferred embodiment of the present invention, a method for preparing a photocurable 3D printing ceramic slurry comprises the following steps:

[0050] (1) Preparation of modified ceramic powder:

[0051] Add part of the dispersant to the anhydrous ethanol solution and perform magnetic stirring to ensure full dissolution, then add the ceramic powder to the anhydrous ethanol solution and stir to react for 1-5 hours (heating may be performed), and after the reaction is completed, perform rotary evaporation to obtain the modified ceramic powder;

[0052] (2) Preparation of primary ceramic slurry:

[0053] The modified ceramic powder obtained in step (1), the ball milling medium, the active diluent, the active monomer and the photoinitiator are mixed, and then ball milled at room temperature for 0.5-2h to obtain a primary ceramic slurry;

[0054] (3) Preparation of ceramic slurry:

[0055] The remaining dispersant is dissolved in anhydrous ethanol to form a dispersant solution, and the dispersant solution is added to the primary ceramic slurry, and ball milling is continued for 0.5-1h to finally obtain a ceramic slurry.

[0056] The third aspect of the present invention provides a photocurable 3D printing ceramic slurry obtained by the preparation method described in the second aspect.

[0057] The fourth aspect of the present invention provides a porous ceramic skeleton made from the photocurable 3D printing ceramic slurry described in the first aspect or the third aspect.

[0058] The porous ceramic skeleton can be prepared by the following method: add the prepared ceramic slurry into a light-curing 3D printer, such as the Austrian printer Lithoz, set the exposure energy and exposure time, and print layer by layer. After printing, place the green body in a degreasing sintering furnace, such as the Hefei Kejing degreasing sintering furnace KSL-1700, and finally obtain the sintered porous ceramic skeleton.

[0059] In order to verify the printability of the ceramic slurry prepared by the present invention, a complex structure ceramic part is formed by a photocuring printer and the final product is obtained by a degreasing and sintering process. Specifically, the ceramic slurry is added to the printer tank, a top-pull printer is used to prepare a ceramic body, and a ceramic product is obtained by degreasing and sintering;

[0060] The degreasing process is at 0-600°C, the heating rate is controlled at 0.1-1°C / min, and the insulation time is 2-10h.

[0061] The sintering process is at 0-1500°C, the heating rate is controlled at 1-5°C / min, and the insulation time is 2-4h.

[0062] The fifth aspect of the present invention provides the use of the porous ceramic skeleton described in the fourth aspect in the preparation of ceramic catalyst carriers and bioceramic implants.

[0063] The present invention will be described in detail below through examples.

[0064] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0065] Example 1

[0066] This example is used to illustrate the preparation of zirconia ceramic slurry.

[0067] (1) 0.3 g of polymer hyperdispersant BYK111 was weighed using an electronic balance (accuracy 0.1 mg) and added to 100 mL of anhydrous ethanol, and magnetically stirred until dissolved to obtain a mixed solution 1; then 30 g of zirconia ceramic powder was added to the mixed solution 1 and magnetically stirred for 2 h, dried and sieved to obtain a modified zirconia powder; wherein the 30 g of zirconia ceramic powder included 3 g (10%) of powder with an average particle size of 4 μm, 6 g (20%) of powder with an average particle size of 1 μm, and 21 g (70%) of powder with an average particle size of 0.2 μm;

[0068] (2) 30 g of modified zirconium oxide powder, 0.1 g of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 3 g of acryloylmorpholine and 4 g of polyethylene glycol diacrylate were mixed, and the mixture was subjected to planetary ball milling at room temperature for 0.5 h to obtain a primary zirconium oxide ceramic slurry;

[0069] (3) 2 g of polymer hyperdispersant BYK111 was weighed and dissolved in 10 mL of anhydrous ethanol at 60° C. The solution was magnetically stirred to form a dispersant solution. The dispersant solution was mixed with the primary zirconia ceramic slurry and ball-milled for 1 h to obtain the zirconia ceramic slurry.

[0070] Comparative Example 1

[0071] Zirconia ceramic slurry was prepared according to the method of Example 1, except that the average particle size of 30 g of zirconia ceramic powder was 0.2 μm.

[0072] Example 2

[0073] This example is used to illustrate the preparation of zirconia ceramic slurry.

[0074] (1) 13.5 g of polymer hyperdispersant BYK-2205 was weighed using an electronic balance (accuracy 0.1 mg) and added to 300 mL of anhydrous ethanol, and magnetically stirred until dissolved to obtain a mixed solution 1; then 270 g of zirconia ceramic powder was added to the mixed solution 1, heated under magnetic stirring for 5 h, dried and sieved to obtain a modified zirconia powder; wherein the 270 g of zirconia ceramic powder included 54 g (20%) of powder with an average particle size of 4 μm, 54 g (20%) of powder with an average particle size of 1 μm, and 162 g (60%) of powder with an average particle size of 0.2 μm;

[0075] (2) 270 g of modified zirconium oxide powder, 1 g of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 35 g of 1,6-hexanediol dimethacrylate and 20 g of polyethylene glycol diacrylate were mixed, and the mixture was subjected to planetary ball milling at room temperature for 2 h to obtain a primary zirconium oxide ceramic slurry;

[0076] (3) Weigh 2 g of polymer superdispersant BYK-2205, dissolve it in 10 mL of anhydrous ethanol at 60° C., and stir it magnetically to form a dispersant solution. The dispersant solution is mixed with the zirconia primary ceramic slurry and ball-milled for 0.5 h to obtain the zirconia ceramic slurry.

[0077] Comparative Example 2

[0078] Zirconia ceramic slurry was prepared according to the method of Example 2, except that the average particle size of 270 g of zirconia ceramic powder was 1 μm.

[0079] Example 3

[0080] This example is used to illustrate the preparation of alumina ceramic slurry.

[0081] (1) 1.8 g of polymer hyperdispersant BYK-110 was weighed using an electronic balance (accuracy 0.1 mg) and added to 200 mL of anhydrous ethanol, and magnetically stirred until dissolved to obtain a mixed solution 1; then 60 g of alumina ceramic powder was added to the mixed solution 1, heated under magnetic stirring for 3 h, dried and sieved to obtain a modified alumina powder; wherein the 60 g of alumina ceramic powder included 15 g (25%) of powder with an average particle size of 4 μm, 6 g (10%) of powder with an average particle size of 1 μm, and 39 g (65%) of powder with an average particle size of 0.2 μm;

[0082] (2) 60 g of modified alumina powder, 0.1 g of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 10 g of isobornyl acrylate and 5 g of polyethylene glycol diacrylate were mixed, and the mixture was subjected to planetary ball milling at room temperature for 1 h to obtain a primary alumina ceramic slurry;

[0083] (3) Weigh 2 g of polymer hyperdispersant BYK-110, dissolve it in 10 mL of anhydrous ethanol at 60° C., and stir it magnetically to form a dispersant solution. The dispersant solution and the alumina primary ceramic slurry are mixed and ball-milled for 1 h to obtain an alumina ceramic slurry.

[0084] Comparative Example 3

[0085] Alumina ceramic slurry was prepared according to the method of Example 3, except that the average particle size of 60 g of alumina ceramic powder was 1 μm.

[0086] Example 4

[0087] This example is used to illustrate the preparation of barium titanate ceramic slurry.

[0088] (1) 1.5 g of polymer hyperdispersant BYK-111 was weighed using an electronic balance (accuracy 0.1 mg) and added to 200 mL of anhydrous ethanol, and magnetically stirred until dissolved to obtain a mixed solution 1; then 50 g of barium titanate ceramic powder was added to the mixed solution 1 and magnetically stirred for 3 h, and dried and sieved to obtain a modified barium titanate powder; wherein the above 50 g of barium titanate ceramic powder included 10 g (20%) of powder with an average particle size of 4 μm, 15 g (30%) of powder with an average particle size of 1 μm, and 25 g (50%) of powder with an average particle size of 0.2 μm;

[0089] (2) 50 g of modified barium titanate powder, 0.1 g of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 6 g of β-hydroxyethyl methacrylate and 7 g of polyethylene glycol diacrylate were mixed, and the mixture was subjected to planetary ball milling at room temperature for 1 h to obtain a primary ceramic slurry of barium titanate;

[0090] (3) 1 g of polymer superdispersant BYK-111 was weighed and dissolved in 5 mL of anhydrous ethanol at 60° C. The solution was magnetically stirred to form a dispersant solution. The dispersant solution was mixed with the barium titanate primary ceramic slurry and ball-milled for 1 h to obtain the barium titanate ceramic slurry.

[0091] Comparative Example 4

[0092] Barium titanate ceramic slurry was prepared according to the method of Example 4, except that the average particle size of the barium titanate ceramic powder was 0.2 μm.

[0093] Example 5

[0094] Zirconia ceramic slurry is prepared according to the method of Example 1, except that in step (1), 30 g of zirconia ceramic powder includes 1.5 g (5%) of powder with an average particle size of 4 μm, 12 g (40%) of powder with an average particle size of 1 μm and 16.5 g (55%) of powder with an average particle size of 0.2 μm.

[0095] Comparative Example 5

[0096] Zirconia ceramic slurry was prepared according to the method of Example 5, except that the average particle size of the zirconia ceramic powder was 0.2 μm.

[0097] Example 6

[0098] Zirconia ceramic slurry is prepared according to the method of Example 1, except that in step (1), 30 g of zirconia ceramic powder includes 6 g (20%) of powder with an average particle size of 4 μm, 9 g (30%) of powder with an average particle size of 1 μm and 15 g (50%) of powder with an average particle size of 0.2 μm.

[0099] Comparative Example 6

[0100] Zirconia ceramic slurry was prepared according to the method of Example 6, except that the average particle size of the zirconia ceramic powder was 1 μm.

[0101] Example 7

[0102] Zirconia ceramic slurry is prepared according to the method of Example 2, except that in step (1), 270 g of zirconia ceramic powder includes 27 g (10%) of powder with an average particle size of 4 μm, 54 g (20%) of powder with an average particle size of 1 μm and 189 g (70%) of powder with an average particle size of 0.2 μm.

[0103] Comparative Example 7

[0104] Barium titanate ceramic slurry was prepared according to the method of Example 4, except that the average particle size of the barium titanate ceramic powder was 1 μm.

[0105] Comparative Example 8

[0106] Barium titanate ceramic slurry was prepared according to the method of Example 4, except that the barium titanate ceramic powder included 5 g (10%) of powder with an average particle size of 1 μm and 45 g (90%) of powder with an average particle size of 0.2 μm.

[0107] Comparative Example 9

[0108] Barium titanate ceramic slurry was prepared according to the method of Example 4, except that the barium titanate ceramic powder included 2.5 g (5%) of powder with an average particle size of 4 μm, 2.5 g (5%) of powder with an average particle size of 1 μm and 45 g (90%) of powder with an average particle size of 0.2 μm.

[0109] Application Examples

[0110] First, the 3D model stl file is imported into the printer and sliced, and the ceramic slurry prepared in the above embodiments and comparative examples is added into the printer material tank, and a ceramic green body is prepared by a layer-by-layer curing method. The green body is placed in a tubular furnace and the heating rate is controlled at 0.2°C / min, and it is kept at 600°C for 2h. The degreased sample is taken out and placed in a muffle furnace and heated to 1450°C at 3°C / min and kept for 2h, and then cooled with the furnace to obtain the corresponding zirconia ceramic products, alumina ceramic products or barium titanate ceramic products.

[0111] Test Example 1

[0112] In this test, the viscosity of the ceramic slurry was tested using the MCR92 rotational rheometer from Anton Paar. The rotor model used in the test was PP-50 (rotor plate diameter 50 mm), the gap height between the rotor and the platform was 1 mm, and the shear rate was 0.1-100 s -1 , the shear rate for data collection is 20s-1 The viscosity value is at an ambient temperature of 25°C.

[0113] In this test, the solid content test was conducted using a DTG-60H differential thermal / thermogravimetric simultaneous analyzer from Shimadzu Corporation of Japan. The thermogravimetric analysis of the photocurable 3D printed ceramic slurry was performed to study the thermal decomposition of organic matter in the slurry. The test temperature range was 25-700°C, the heating rate was 10°C / min, and the holding time was 1h.

[0114] The results are shown in Table 1.

[0115] Table 1

[0116]

[0117]

[0118] It can be seen from the results in Table 1 that the present invention reasonably grades the particle size of the ceramic powder for preparing the ceramic slurry, thereby ensuring the solid content at a high level while greatly reducing the slurry viscosity, thereby ensuring the flowability and forming properties of the ceramic slurry.

[0119] Compared with commercial photocurable ceramic slurry, the present invention can prepare ceramic slurry with lower viscosity, and the preparation process is simple and easy to implement, and the preparation cycle is short. The ceramic slurry combined with a photocurable 3D printer can successfully print ceramic green bodies with complex structures, and after degreasing and sintering processes, complex ceramic parts are finally obtained.

[0120] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A photocurable 3D printing ceramic slurry, characterized in that: The ceramic slurry includes ceramic powder; The ceramic powder comprises the following components by mass percentage: 5-25% of ceramic powder with an average particle size of 4 μm, 10-40% of ceramic powder with an average particle size of 1 μm, and 40-80% of ceramic powder with an average particle size of 0.2 μm.

2. The ceramic slurry according to claim 1, wherein The ceramic powder comprises the following components by mass percentage: 10-20% of ceramic powder with an average particle size of 4 μm, 20-30% of ceramic powder with an average particle size of 1 μm, and 50-70% of ceramic powder with an average particle size of 0.2 μm; Preferably, the ceramic powder comprises the following components by mass percentage: 20% of ceramic powder with an average particle size of 4 μm, 30% of ceramic powder with an average particle size of 1 μm, and 50% of ceramic powder with an average particle size of 0.2 μm.

3. The ceramic slurry according to claim 1 or 2, wherein: The ceramic slurry also includes a photoinitiator, a reactive diluent, a reactive monomer and a dispersant; Preferably, the ceramic slurry comprises the following components by mass percentage: 70-80% ceramic powder, 0.1-1% photoinitiator, 5-15% active diluent, 10-20% active monomer and 1-6% dispersant.

4. The ceramic slurry according to any one of claims 1 to 3, wherein The material of the ceramic powder is selected from at least one of silicon oxide, aluminum oxide, zirconium oxide, barium titanate, silicon carbide and silicon nitride; Preferably, the photoinitiator is selected from at least one of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, bis-2,6-difluoro-3-pyrrolophenyl titanocene, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and a,a-dimethoxy-a-phenylacetophenone; Preferably, the reactive diluent is selected from at least one of isobornyl acrylate, acryloyl morpholine, β-hydroxyethyl methacrylate, 1,6-hexanediol diacrylate, tridecyl acrylate, dodecyl methacrylate, lauryl acrylate and 1,6-hexanediol dimethacrylate; Preferably, the active monomer is selected from at least one of polyethylene glycol diacrylate, diethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate and ethoxylated pentaerythritol tetraacrylate; Preferably, the dispersant is selected from at least one of polymer hyperdispersants.

5. A method for preparing a photocurable 3D printing ceramic slurry according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) mixing a portion of the dispersant with the ceramic powder and reacting the mixture to obtain a modified ceramic powder; (2) mixing the modified ceramic powder obtained in step (1) with a reactive diluent, a reactive monomer and a photoinitiator, and then performing a first ball milling to obtain a primary ceramic slurry; (3) The primary ceramic slurry obtained in step (2) is mixed with the remaining dispersant and then subjected to a second ball milling to obtain the ceramic slurry.

6. The preparation method according to claim 5, wherein: The mass ratio of the part of the dispersant described in step (1) to the remaining dispersant described in step (3) is 0.3-13.5:2, preferably 1.8-3:

2.

7. The preparation method according to claim 5 or 6, wherein: The reaction time of step (1) is 1-5h; Preferably, the first ball milling time in step (2) is 0.5-2h; Preferably, the time of the second ball milling in step (3) is 0.5-1 h.

8. A photocurable 3D printing ceramic slurry obtained by the preparation method according to any one of claims 5 to 7.

9. A porous ceramic skeleton made from the photocurable 3D printing ceramic slurry according to claim 1 or 8.

10. Use of the porous ceramic skeleton according to claim 9 in the preparation of ceramic catalyst carriers and bioceramic implants.

Citation Information

Patent Citations

  • Ultralow-viscosity light-cured ceramic resin slurry

    CN112142452A

  • Ceramic slurry and preparation method and application thereof

    CN112479723A

  • Two-step sintering method based on 3D printing SiC-SiO2 ceramic green body

    CN114276143A

  • Silicon-based ceramic slurry for photocuring 3D printing and preparation method of silicon-based ceramic slurry

    CN117383915A

  • Production of ceramic

    JP1998130061A