Thermoplastic methyl methacrylate resin system, thermoplastic FRP (Fiber Reinforced Plastic) embossed rib and production process of thermoplastic FRP embossed rib

Through low viscosity thermoplastic methyl methacrylate resin system and multi-zone temperature control technology of pultruding mold, combined with the winding embossing belt process, the recovery of thermosetting resin-based composite materials and the preparation of thermoplastic resin-based composite materials are solved, achieving high efficiency , low energy consumption to produce high-performance thermoplastic FRP embossed ribs.

CN118909201APending Publication Date: 2024-11-08ZHONGFU CARBON FIBER CORE CABLE TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411004076.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing thermosetting resin-based composite ribs cannot be recycled and reused, the preparation process is complex and energy-consuming, the thermoplastic resin-based composite ribs have low fiber content, small specifications, and a single shape. The existing thermoplastic methyl methacrylate resin system is difficult to dissolve. This results in low mechanical properties of resin matrix and cannot produce large-scale and low-energy consumption.

Method used

Using a low viscosity thermoplastic methyl methacrylate resin system, including thermoplastic acrylate mixture, initiator, plasticizer, internal mold release agent and compound additive, prepolymerization and cooling through room temperature mixing, combining with the multi-purification mold Zone temperature control and winding embossing tape technology to prepare thermoplastic FRP embossing ribs with high fiber content and low defects.

Benefits of technology

High-efficiency production of high-performance corrosion-resistant thermoplastic FRP embossing ribs with large diameter, high fiber content and low defects is achieved, the preparation process is simplified, the curing temperature and energy consumption are reduced, and the fiber wetting effect and mechanical properties are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909201A_ABST
    Figure CN118909201A_ABST
Patent Text Reader

Abstract

The invention discloses a thermoplastic methyl methacrylate resin system, a thermoplastic FRP (Fiber Reinforced Plastic) embossed rib and a production process thereof, particularly relates to the technical field of preparation of resin-based composite materials, and aims to solve the problems that high-temperature curing is mostly needed in the preparation process of ribbed FRP ribs in the prior art, and efficient production cannot be realized while high-quality production is ensured. The thermoplastic FRP embossed rib comprises a thermoplastic methyl methacrylate resin system, the resin system comprises, by mass, 100 parts of a thermoplastic acrylate mixture, 0.5-3 parts of an initiator, 2-15 parts of a plasticizer, 1-3 parts of an internal release agent and 0.5-3 parts of a compound auxiliary agent, and the invention further provides a production process for preparing the thermoplastic FRP embossed rib by using the resin system. According to the invention, high-efficiency production of the high-performance corrosion-resistant thermoplastic FRP embossed rib with large diameter, high fiber content and low defect can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a thermoplastic methyl methacrylate resin system, a thermoplastic FRP embossed rib and a production process thereof, and belongs to the technical field of preparation of resin-based composite materials. Background Art

[0002] Fiber-reinforced thermosetting resin-based composite ribs have a simple molding process, good mechanical properties, and are widely used, but they cannot be recycled and reused, and their shape cannot be changed after they are produced. Fiber-reinforced thermoplastic resin-based composite ribs have higher toughness, greater impact strength, can be secondary molded, and are recyclable. However, thermoplastic resins such as polyamide, polycarbonate, and polyvinyl chloride have high viscosities, and higher temperatures and pressures are required when preparing composite materials, resulting in complex molding processes and high energy consumption. The finished products have low fiber content, small specifications, and a single shape. Therefore, thermoplastic resin-based composite ribs have not been widely promoted and applied.

[0003] Thermoplastic modified methyl methacrylate resin has low molecular weight, low viscosity and excellent process performance, providing a new way for fiber-reinforced thermoplastic resin composite rib forming. Publication No. CN116589639A proposes a thermoplastic methyl methacrylate resin system and a method for in-situ injection pultrusion of fiber-reinforced materials, but in practice, it is difficult to dissolve polymethyl methacrylate particles in acrylate, resulting in low mechanical properties of the resin matrix, and still requires high temperature curing at 80-180°C, which cannot be produced on a large scale, long-term and with low energy consumption.

[0004] At present, most of the ribbed FRP (fiber reinforced composite material) bars developed at home and abroad use fiber reinforced thermosetting resin composite materials, and the shape and geometric dimensions of the ribbed FRP bars prepared by them are fixed and cannot be prepared continuously. Some studies use epoxy resin curing and bonding methods to prepare ribbed FRP bars. This method has problems such as low bonding strength between the bars and ribs and easy debonding. A small number of studies use mechanical methods to form a threaded structure on the surface of the FRP bars, which increases the surface area of ​​the FRP bars. However, this method causes partial fiber breakage on the surface, which significantly reduces the mechanical properties and durability. A very small number of studies use thermoplastic resin ribs to wrap FRP bars, but their rib forming process still uses the traditional thermosetting rib forming method, which does not really give play to the advantages of thermoplastic resins that can be melted and formed twice.

[0005] Publication No. CN117447802A proposes a thermoplastic methyl acrylate resin system and its thermoplastic composite rib and preparation method. Auxiliary equipment such as a glue injection machine and a glue injection box are required. The equipment investment cost is high and the production speed is slow. In addition, the method of making the embossed rib is to form a smooth round rib by in-situ polymerization in a mold. After the smooth round rib leaves the die, a rib pressing device is used to press and form ribs on the surface of the smooth round rib to prepare a thermoplastic composite rib. The embossing is performed by machine pressing, which can easily damage or break some fibers, thereby reducing their mechanical properties.

[0006] In addition, the current domestic production of thermoplastic reinforcement has low production efficiency and cannot achieve large-scale production. Summary of the invention

[0007] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a thermoplastic methyl methacrylate resin system, a thermoplastic FRP embossed rib and a production process thereof, which can realize the efficient production of high-performance corrosion-resistant thermoplastic FRP embossed ribs with large diameter, high fiber content and low defects.

[0008] To achieve the above object, the present invention is implemented by adopting the following technical solutions: In a first aspect, the present invention provides a thermoplastic methyl methacrylate resin system, wherein the viscosity of the thermoplastic methyl methacrylate resin system is 500-1200 mPa·S, and the system comprises, by mass, 100 parts of a thermoplastic acrylate mixture, 0.5-3 parts of an initiator, 2-15 parts of a plasticizer, 1-3 parts of an internal mold release agent, and 0.5-3 parts of a compounding auxiliary agent; the main components of the internal mold release agent are organic fatty acids, esters, amines, and the like.

[0009] The thermoplastic acrylic ester mixture is a methyl methacrylate-ethyl acrylate copolymer dissolved in methyl methacrylate, and its viscosity is 400-600 mPa·S.

[0010] Optionally, the initiator is one or more of dodecyl peroxide, tert-butyl perbenzoate, N,N-dimethyl-p-toluidine, dibenzoyl peroxide, and azobisisobutyronitrile.

[0011] Optionally, the plasticizer includes one or more of dibutyl phthalate, dioctyl phthalate, triphenyl phosphate, tributyl phosphate, dioctyl adipate, and diisononyl adipate.

[0012] Optionally, the compounding auxiliary agent includes 0-3 parts of N,N-dimethylaniline and 0.5-3 parts of an exothermic peak reducing auxiliary agent by weight. Adding the compounding auxiliary agent can reduce the exothermic peak of the pultrusion process, reduce the temperature required for curing, and enable the FRP embossed ribs to cure more quickly.

[0013] In a second aspect, the present invention provides a production process of a thermoplastic methyl methacrylate resin system, which is used to prepare any of the above-mentioned thermoplastic methyl methacrylate resin systems, comprising: The thermoplastic acrylate mixture, initiator, plasticizer, internal mold release agent and compounding auxiliary agent are uniformly mixed at room temperature, and then prepolymerized and cooled to obtain a thermoplastic methyl methacrylate resin system.

[0014] Furthermore, the prepolymerization includes prepolymerization at 40-80°C for 10-60 min, and the cooling is performed at 0-10°C.

[0015] In a third aspect, the present invention provides a production process for thermoplastic FRP embossed ribs, comprising: Dipping the fiber filaments into the thermoplastic methyl methacrylate resin system as described in any one of the above items to obtain dipped fiber filaments; Bundling the impregnated fiber strands into fiber bundles; Winding an embossed tape on the surface of the fiber bundle to obtain a fiber bundle with the embossed tape wound on the surface; The fiber bundle with the embossed tape wrapped around the surface is pulled and cured by heating, and the thermoplastic FRP embossed ribs are obtained after the embossed tape is torn off.

[0016] Furthermore, the temperature rise curing adopts a pultrusion die, the pultrusion speed is 200~400mm / min, the pultrusion die is divided into 4 temperature zones from the die inlet to the die outlet, and the temperature zones include a first temperature zone, a second temperature zone, a third temperature zone and a fourth temperature zone, wherein the first temperature zone is 50~80°C, the second temperature zone is 100~130°C, the third temperature zone is 80~120°C, and the fourth temperature zone is 14~20°C.

[0017] Furthermore, the total length of the pultrusion die is 1000 mm, wherein the length of the first temperature zone is 200 mm, the length of the second temperature zone is 300 mm, the length of the third temperature zone is 300 mm, and the length of the fourth temperature zone is 200 mm.

[0018] In a fourth aspect, the present invention further provides a thermoplastic FRP embossed rib, which is prepared by the production process of the thermoplastic FRP embossed rib described in any one of the above items.

[0019] Compared with the prior art, the present invention has the following beneficial effects: The thermoplastic methyl methacrylate resin system provided by the present invention has low viscosity and is stored in a liquid state at room temperature. It does not need to be dissolved in advance before use, which is convenient for use and improves the fiber impregnation effect. Even in the case of large diameter (diameter ≥ 20 mm) and high fiber content, the fiber surface can be fully impregnated without defects. The preparation process of the thermoplastic methyl methacrylate resin system does not require high temperature and pressure, and the preparation process is simple. When preparing thermoplastic FRP embossed ribs, the embossed tape is added before the pultrusion die and is torn off after curing. The fibers are only slightly bent but not damaged, thereby ensuring higher tensile strength and modulus. Moreover, the embossing depth on the surface of the FRP embossed ribs can be adjusted according to the depth change of the embossed tape, thereby adjusting the embossing depth according to product performance requirements, which is simple and convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A schematic diagram of the structure of a thermoplastic FRP embossed rib in an embodiment of the present invention; Figure 2 It is a schematic structural diagram of a production device used in a production process of plastic FRP embossed ribs in one embodiment of the present invention; In the figure: 1 FRP embossed rib, 2 FRP embossed rib embossing, 3 FRP embossed rib pitch, 4 yarn rack, 5 yarn comb, 6 V-shaped sunken resin glue tank, 7 pre-curing mold, 8 first glue extrusion hole, 9 second glue extrusion hole, 10 embossed belt and fiber bundle angle, 11 winding disk, 12 winding machine, 13 rotating disk, 14 pultrusion mold, 15 water circulation device, 16 unwinding machine, 17 traction machine, 18 cutting machine. DETAILED DESCRIPTION

[0021] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.

[0022] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article.

[0023] For the purpose of this specification and the appended claims, unless otherwise stated, all numbers expressing amounts, percentages or ratios and other numerical values ​​used in this specification and the appended claims are understood to be modified in all cases by the term "about". In addition, all ranges disclosed herein are inclusive and independently combinable. Example 1

[0024] The present embodiment provides a thermoplastic methyl methacrylate resin system, which includes, by weight, 100 parts of a thermoplastic acrylate mixture, 1 part of an initiator (dodecyl peroxide), 8 parts of a plasticizer (dioctyl phthalate), 2 parts of an internal release agent and 0.5 parts of a compounding auxiliary agent, wherein the compounding auxiliary agent is composed of 0.2 parts of N,N-dimethylaniline and 0.3 parts of an exothermic peak reducing auxiliary agent.

[0025] The thermoplastic acrylate mixture used is Elium C595E, the internal mold release agent is INT-PUL24, the manufacturer is AXEL, the compounding additive is BYK-P_9929, the manufacturer is BYK Chemical. The exothermic peak reducing additive is BYK-P_9929, the manufacturer is BYK Chemical. Example 2

[0026] This embodiment provides a thermoplastic methyl methacrylate resin system, which is different from Embodiment 1 only in that 1.5 parts of compounding auxiliary agents are included, and the compounding auxiliary agents are composed of 0.6 parts of N,N-dimethylaniline and 0.9 parts of an auxiliary agent for reducing the exothermic peak.

[0027] Comparative Example 1: This comparative example provides a common thermoplastic resin with a brand name of Elium C595E, a batch number of A104230318, and a manufacturer of ARKEMA. Example 3

[0028] The invention provides a production process of a thermoplastic methyl methacrylate resin system, comprising the steps of uniformly mixing a thermoplastic acrylate mixture, an initiator, a plasticizer, an internal mold release agent and a compounding auxiliary agent at room temperature, prepolymerizing the mixture at 40°C for 10 minutes, and rapidly cooling the mixture at 0°C to obtain the thermoplastic methyl methacrylate resin system. Example 4

[0029] The invention provides a production process of a thermoplastic methyl methacrylate resin system, comprising the steps of uniformly mixing a thermoplastic acrylate mixture, an initiator, a plasticizer, an internal mold release agent and a compounding auxiliary agent at room temperature, prepolymerizing the mixture at 60°C for 34 minutes, and rapidly cooling the mixture at 5°C to obtain the thermoplastic methyl methacrylate resin system. Example 5

[0030] The invention provides a production process of a thermoplastic methyl methacrylate resin system, comprising the steps of uniformly mixing a thermoplastic acrylate mixture, an initiator, a plasticizer, an internal mold release agent and a compounding auxiliary agent at room temperature, prepolymerizing the mixture at 80°C for 60 minutes, and rapidly cooling the mixture at 10°C to obtain the thermoplastic methyl methacrylate resin system. Example 6

[0031] This embodiment also provides a production device for thermoplastic FRP embossed ribs, such as Figure 2 As shown, the production device includes a yarn rack, a V-shaped sunken resin glue groove, a pre-curing mold, a first glue extrusion hole, a second glue extrusion hole, a winding disk, a rotating disk, a pultrusion mold, an unwinder, a traction machine, and a cutting machine, which are arranged in sequence, and the winding disk is controlled by the winding machine.

[0032] The use of a V-shaped sunken resin glue groove can make the fibers easier to twist, further improving the fiber impregnation effect, and is equipped with a first glue extrusion hole and a second glue extrusion hole to reduce the amount of resin on the fiber before entering the mold, avoiding the situation where most of the resin accumulates at the mold mouth due to the residual temperature of the mold mouth. There is no need for additional auxiliary equipment such as glue injection machines, which greatly reduces production investment costs.

[0033] A yarn comb is arranged between the yarn frame and the V-shaped sunken resin adhesive groove, so that multiple fiber filaments are evenly arranged into the V-shaped sunken resin adhesive groove, and the pre-curing mold is used to bundle the fiber filaments into fiber bundles. Example 7

[0034] Based on Example 6, this example provides a production process for preparing thermoplastic FRP embossed ribs, comprising the following steps: Step 1: prepare a predetermined number of fiber filaments, which are ordinary glass fibers. Install a predetermined number of fiber filaments on the yarn frame according to the designed arrangement so that the fibers can be drawn out from the yarn guide holes neatly and evenly. Use a tension meter to measure the tension of each fiber and keep it consistent. Then the fibers are evenly arranged and passed through the yarn comb. Under the action of traction, the fiber yarns enter the V-shaped sunken glue tank for dipping. Compared with injection pultrusion, no additional auxiliary equipment such as glue injection machines is required. The glue is a thermoplastic methyl methacrylate resin system.

[0035] Step 2: The resin-impregnated fiber yarn passes through a pre-curing mold to bundle the resin-impregnated fiber yarn into a fiber bundle, and then passes through a first extrusion hole and a second extrusion hole in sequence, and the extruded resin glue flows back into the V-shaped sunken resin glue tank.

[0036] Step 3: The fiber bundle then passes through the center of the rotating disk, and the winding machine starts working, winding the embossed tape on the surface of the fiber bundle. By adjusting the thickness and width of the wound embossed tape, the embossing depth and width of the anchor rod are controlled; by adjusting the motor frequency of the winding machine, the pitch of the embossing on the surface of the reinforcement is controlled; by controlling the angle of the winding disk, the embossed tape is adjusted to form an angle α with the axis of the fiber bundle. The value range of α is 50°~70°. In this embodiment, the value of α is 60°. This angle can make the embossed tape better fit the chamfer of the mold entrance when rotating into the mold, and enter the mold more smoothly, so that the surface texture of the FRP embossed reinforcement is uniform when it is out of the mold.

[0037] Step 4: The fiber bundle with the embossed tape wrapped on the surface is pulled into the pultrusion die by a traction machine for curing, and can be shaped into a thermoplastic FRP embossed rib with a continuous threaded surface. In this embodiment, the fiber bundle and the embossed tape wrapped on the surface enter the mold together, are in close contact with the shaping mold, and are cured and formed in the mold. The product after demolding is consistent with the mold cross-section, standard in size, and high in precision, which is different from the traditional wound FRP threaded rib.

[0038] In this embodiment, the length of the pultrusion die is 1000 mm, which is divided into four temperature zones, wherein the length of the first temperature zone is 200 mm, the length of the second temperature zone is 300 mm, the length of the third temperature zone is 300 mm, and the length of the fourth temperature zone is 200 mm.

[0039] The temperature of the pultrusion die is set according to the curing temperature of the resin glue. The first temperature zone is 50~80℃, the second temperature zone is 100~130℃, the third temperature zone is 80~120℃, and the fourth temperature zone is 14~20℃.

[0040] A cold water circulation device is added to the end of the pultrusion die (i.e., the fourth temperature zone) to make the die temperature drop suddenly, thereby achieving the effect of rapid pultrusion of thermoplastic resin. Due to the characteristics of thermoplastic resin, if the pultrusion speed is increased without increasing the temperature, the reinforcement material will not be solidified after leaving the die; if the temperature is increased at the same time, the reinforcement material will dissolve again after solidification, resulting in a very poor appearance. If you want to achieve the purpose of high-speed pultrusion, you need to lengthen the die without increasing the curing temperature, which will greatly increase the production cost. Therefore, the best balance point is found by rapid heating and cooling. After heating and curing, it is immediately cooled to ensure that the reinforcement material will not dissolve, so as to achieve the purpose of high-speed pultrusion.

[0041] Step 5: After the FPR embossed ribs are completely cured by the curing mold, they are unwound by the unwinding machine. The embossed tape wrapped around the surface of the FRP embossed ribs when entering the mold is wound off. The embossed tape is added before entering the mold and torn off after curing. The fiber is only slightly bent, but not damaged, which can ensure higher tensile strength and modulus. It can also make the fiber tightly squeezed with the curing mold, and it is completely cured after leaving the mold, so that the size of the prepared FRP embossed ribs is more accurate.

[0042] The fiber bundles torn off the embossed tape pass through a traction machine, under the action of which the FRP embossed ribs with continuous threads on the surface are conveyed to a cutting machine, where the FRP embossed ribs are cut to a fixed length.

[0043] The prepared thermoplastic FRP embossed ribs are Figure 1 As shown, staggered embossing and ribs are provided on its surface.

[0044] The following is a performance analysis of the thermoplastic resin system of Examples 1, 2 and Comparative Example 1. Examples 1 and 2 use the process described in Example 5 to prepare thermoplastic resins, and then use the production process described in Example 7 to obtain thermoplastic FRP embossed ribs. Comparative Example 1 uses a conventional process method in the prior art.

[0045] The specific condition parameters of the process scheme of Examples 1, 2 and Comparative Example 1 are shown in Table 1: Table 1: Preparation of thermoplastic FRP embossed ribs by thermoplastic resin systems of Examples 1, 2 and Comparative Example 1

[0046] The fiber volume content refers to the volume percentage of the fiber in the cross section of the thermoplastic FRP embossed rib, and the rest is resin. The higher the fiber volume content, the better the mechanical properties of the thermoplastic FRP embossed rib.

[0047] The properties of the thermoplastic FRP embossed ribs numbered 1 to 5 in Table 1 are shown in Table 2.

[0048] Table 2: Performance of thermoplastic FRP embossed bars No. 1 to 5

[0049] Among them, the test method of dyeing permeability is to cut a slice of FRP embossed rib, put it into a fuchsin solution, and observe the situation of the fuchsin solution penetrating into the interior of the slice. If the dyeing permeability is higher, it means that the internal porosity of the FRP embossed rib is larger, and there may be cracks inside.

[0050] The performance of FRP embossed ribs of No. 1 and No. 2 is compared by combining the data in Table 1 and Table 2. Since the performance of No. 2 is better than that of No. 1, it can be seen that the resin system formula of Example 2 is better than that of Example 1.

[0051] Comparing the performance of FRP embossed ribs No. 2 and No. 3, the performance of No. 2 is also better than that of No. 3, which shows that the pultrusion speed cannot be too fast when preparing FRP embossed ribs, which may easily lead to the rib material failing to solidify after leaving the mold.

[0052] Comparing the performance of FRP embossed ribs of No. 3 and No. 4, the performance of No. 4 is also better than that of No. 3. This shows that a water cooling device is provided at the end of the pultrusion die, which lowers the fourth temperature zone and finds the best balance point by rapid heating and cooling. After heating and curing, cooling is performed immediately, which effectively promotes the curing of the rib material and achieves the purpose of high-speed pultrusion.

[0053] The FRP embossed rib No. 5 made of ordinary thermoplastic resin is prepared by using a conventional oven. The conventional oven does not involve pultrusion operation and cannot extrude excess resin. Therefore, the fiber volume content can only reach 65% at most, and its various performance indicators are relatively poor.

[0054] In summary, the optimal formula of the thermoplastic methyl methacrylate resin system includes, by mass, 100 parts of a thermoplastic acrylate mixture, 1 part of an initiator (dodecyl peroxide), 8 parts of a plasticizer (dioctyl phthalate), 2 parts of an internal release agent and 1.5 parts of a compounding auxiliary agent.

[0055] The best temperature zones in the pultrusion die for the production process of preparing FRP embossed ribs are: 70°C in the first temperature zone, 110°C in the second temperature zone, 100°C in the third temperature zone, and 14°C in the fourth temperature zone.

[0056] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A thermoplastic methyl methacrylate resin system, It is characterized in that The viscosity of the thermoplastic methyl methacrylate resin system is 500-1200 mPa·S, and the system comprises, by mass, 100 parts of a thermoplastic acrylate mixture, 0.5-3 parts of an initiator, 2-15 parts of a plasticizer, 1-3 parts of an internal release agent, and 0.5-3 parts of a compounding auxiliary agent; The thermoplastic acrylic ester mixture is a methyl methacrylate-ethyl acrylate copolymer dissolved in methyl methacrylate, and its viscosity is 400-600 mPa·S.

2. The thermoplastic methyl methacrylate resin system according to claim 1, It is characterized in that The initiator is one or more of lauroyl peroxide, tert-butyl perbenzoate, N,N-dimethyl-p-toluidine, dibenzoyl peroxide, and azobisisobutyronitrile.

3. The thermoplastic methyl methacrylate resin system according to claim 1, It is characterized in that The plasticizer includes one or more of dibutyl phthalate, dioctyl phthalate, triphenyl phosphate, tributyl phosphate, dioctyl adipate, and diisononyl adipate.

4. The thermoplastic methyl methacrylate resin system according to claim 1, It is characterized in that The compound auxiliary agent comprises, by weight, 0 to 3 parts of N,N-dimethylaniline and 0.5 to 3 parts of an auxiliary agent for reducing the exothermic peak.

5. A production process for a thermoplastic methyl methacrylate resin system, It is characterized in that It is used to prepare the thermoplastic methyl methacrylate resin system according to any one of claims 1 to 4, comprising: The thermoplastic acrylate mixture, initiator, plasticizer, internal mold release agent and compounding auxiliary agent are uniformly mixed at room temperature, and then prepolymerized and cooled to obtain a thermoplastic methyl methacrylate resin system.

6. The production process of the thermoplastic methyl methacrylate resin system according to claim 5, It is characterized in that The prepolymerization includes prepolymerization at 40-80°C for 10-60 minutes, and the cooling is performed at 0-10°C.

7. A production process for thermoplastic FRP embossed ribs, It is characterized in that It includes: Dipping the fiber filaments in the thermoplastic methyl methacrylate resin system according to any one of claims 1 to 4 to obtain dipped fiber filaments; Bundling the impregnated fiber strands into fiber bundles; Winding an embossed tape on the surface of the fiber bundle to obtain a fiber bundle with the embossed tape wound on the surface; The fiber bundle with the embossed tape wound on the surface is pulled and cured by heating to obtain the thermoplastic FRP embossed rib.

8. The production process of thermoplastic FRP embossed ribs according to claim 7, It is characterized in that The temperature rise curing adopts a pultrusion die, the pultrusion speed is 200~400mm / min, the pultrusion die is divided into 4 temperature zones from the die inlet to the die outlet, and the temperature zones include a first temperature zone, a second temperature zone, a third temperature zone and a fourth temperature zone, wherein the first temperature zone is 50~80°C, the second temperature zone is 100~130°C, the third temperature zone is 80~120°C, and the fourth temperature zone is 14~20°C.

9. The production process of thermoplastic FRP embossed ribs according to claim 8, It is characterized in that The total length of the pultrusion die is 1000 mm, wherein the length of the first temperature zone is 200 mm, the length of the second temperature zone is 300 mm, the length of the third temperature zone is 300 mm, and the length of the fourth temperature zone is 200 mm.

10. A thermoplastic FRP embossed rib, It is characterized in that It is prepared by the production process of thermoplastic FRP embossed ribs described in claim 8.

Citation Information

Patent Citations

  • Thermoplastic methyl methacrylate resin system and method for in-situ injection pultrusion of fiber reinforced material

    CN116589639A

  • Thermoplastic methyl acrylate resin system as well as thermoplastic composite rib and preparation method thereof

    CN117447802A