Core-shell wollastonite-sericite-PCL composite material as well as preparation method and application thereof

By using core-shell wollastonite-sermica-PCL composite in engineering plastics, combined with modified wollastonite-sermica composite and polyε-caprolactone, the mechanical properties of traditional engineering plastics are solved and resistant to resistance. The problem of poor thermal properties has achieved high performance and environmentally friendly composite material preparation.

CN118909231APending Publication Date: 2024-11-08JIANGXI GUANGYUAN CHEM +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411331808.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In long-term use, traditional single engineering plastics have unstable mechanical properties, poor heat and chemical resistance, making it difficult to meet the improvement of industrial demand.

Method used

Using core-shell wollastonite-sermica-PCL composite material, the modified wollastonite-sermica composite is used as the core and polyepsilane-caprolactone as the shell layer, combining silane coupling agent and slurry composite agent The polymerization reaction is carried out to form a composite material with excellent mechanical properties, heat resistance and chemical resistance.

Benefits of technology

It significantly improves the mechanical properties, heat resistance and chemical resistance of composite materials, and has good processing properties and environmentally friendly and non-toxic characteristics, and is suitable for the preparation of engineering plastics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a core-shell wollastonite-sericite-PCL composite material as well as a preparation method and application thereof, and belongs to the technical field of engineering plastics. The preparation method comprises the following steps: firstly, respectively preparing wollastonite powder slurry and sericite powder slurry, then compounding the two types of slurry, modifying by using a silane coupling agent, mixing the obtained modified wollastonite-sericite compound with an organic solvent, epsilon-caprolactone, an initiator and a catalyst, and carrying out melt extrusion to obtain the modified wollastonite-sericite composite material. And carrying out polymerization reaction to obtain the core-shell wollastonite-sericite-PCL composite material. The wollastonite-sericite-PCL composite material prepared by the invention has a core-shell structure taking a modified wollastonite-sericite compound as a core and PCL as a shell, has the advantages of excellent mechanical properties, cheap and easily available raw materials, biodegradability, environmental protection, no toxicity and the like, and can be used in the fields of engineering plastic preparation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering plastics, and in particular to a core-shell type wollastonite-sericite-PCL composite material and a preparation method and application thereof. Background Art

[0002] Wollastonite is a single-chain silicate mineral, the main component of which is Ca3Si3O9, triclinic system, usually in the form of flakes, radial or fibrous aggregates. Due to its special crystal structure, wollastonite has good insulation, high whiteness, good dielectric properties, and is generally resistant to acid, alkali and chemical corrosion. Therefore, wollastonite is widely used in plastics, ceramics, rubber, papermaking, coatings and other fields.

[0003] Sericite is a natural fine-grained white mica, a layered silicate that can be split into extremely thin sheets with a thickness of less than 1μm (theoretically, it can be cut to 0.001μm), with a large diameter-to-thickness ratio, good wear resistance and abrasion resistance, heat resistance and insulation, insoluble in acid and alkali solutions, and stable chemical properties. Sericite has a wide range of uses, including rubber, plastics, coatings, paints, ceramics, thermal insulation, cosmetics, pigments, papermaking, metallurgy and other industries.

[0004] Poly-ε-caprolactone (PCL) is currently an important biodegradable polymer material. It is made of ε-caprolactone as a raw material through ring-opening polymerization under the action of a catalyst. It has a melting point of about 60°C and is a linear polymer. Its repeating unit consists of 1 polar ester group -COO- and 5 non-polar methylene groups -CH2-. The molecular chain is regular and flexible and relatively easy to crystallize. Due to the presence of polar ester groups in the molecular chain of PCL, the lipase released by bacteria or molds widely distributed in the soil can hydrolyze the ester bonds in the polyester, so PCL has good biocompatibility and can be completely biodegraded.

[0005] At present, there are many kinds of engineering plastics on the market, among which polycarbonate (PC), polyamide (PA, nylon), polypropylene (PP) and polyethylene (PE) occupy an important position, showing a wide range of application potential in many fields such as automobile manufacturing, electronic appliances, construction materials, medical equipment, etc. However, with the increasing industrial demand, traditional single-material engineering plastics have gradually exposed their limitations. In the long-term use process, they face problems such as unstable mechanical properties, poor heat resistance and chemical resistance. Therefore, the development of a new composite material that can maintain the advantages of traditional engineering plastics and significantly improve their mechanical properties, heat resistance and chemical resistance has become a research hotspot in the current field of engineering plastics. Summary of the invention

[0006] The object of the present invention is to provide a core-shell wollastonite-sericite-PCL composite material and a preparation method and application thereof, wherein the mechanical properties, heat resistance and chemical resistance of the composite material are improved.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a core-shell type wollastonite-sericite-PCL composite material, comprising the following steps:

[0009] Mixing wollastonite powder, water and a first composite dispersant to obtain wollastonite powder slurry;

[0010] Mixing sericite powder, water and a second composite dispersant to obtain sericite powder slurry;

[0011] The wollastonite powder slurry, the sericite powder slurry and the slurry compounding agent are mixed for compounding, and the obtained composite slurry is sequentially dried, ground and sieved to obtain a wollastonite-sericite composite;

[0012] The wollastonite-sericite composite is mixed with a silane coupling agent and modified to obtain a modified wollastonite-sericite composite;

[0013] The modified wollastonite-sericite composite material, an organic solvent, ε-caprolactone, an initiator and a catalyst are mixed and polymerized to obtain a core-shell type wollastonite-sericite-PCL composite material.

[0014] Preferably, the first composite dispersant is polyethylene glycol fatty acid sodium and sodium dodecyl sulfate, the mass of the first composite dispersant is 5-9‰ of the mass of the wollastonite powder, and the mass ratio of the polyethylene glycol fatty acid sodium to the sodium dodecyl sulfate is 1:4-1:6;

[0015] The second composite dispersant is sodium polyacrylate and sodium stearate, the mass of the second composite dispersant is 5-9‰ of the mass of the sericite powder, and the mass ratio of the sodium polyacrylate to the sodium stearate is 1:4-1:6.

[0016] Preferably, the solid content of the wollastonite powder slurry is 60-65wt%, the solid content of the sericite powder slurry is 55-60wt%, and the solid content of the composite slurry is 65-70wt%.

[0017] Preferably, the slurry compounding agent includes one or more of sodium lignin sulfonate, sodium trifluoromethanesulfinate, 4-aminoazobenzene-4-acid, and 2-naphthylamine-1-sulfonic acid, and the mass of the slurry compounding agent is 4 to 8‰ of the total mass of the wollastonite powder and the sericite powder.

[0018] Preferably, the silane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane, and the mass ratio of the silane coupling agent to the wollastonite-sericite composite is (1-2):(100-120).

[0019] Preferably, the modification temperature is 80-90° C., and the stirring speed is 80-100 r / min.

[0020] Preferably, the mass ratio of the modified wollastonite-sericite composite to the ε-caprolactone is (100-120):(100-200).

[0021] Preferably, the solvent includes one of toluene and dichloromethane, the initiator includes one of propylene glycol, sodium nitrite and aniline, and the mass ratio of the initiator to the ε-caprolactone is 1:(100-200); the catalyst includes one of stannous octoate and stannous chloride, and the mass ratio of the catalyst to the ε-caprolactone is (0.1-0.5):(100-200).

[0022] The present invention also provides a core-shell type wollastonite-sericite-PCL composite material prepared by the above preparation method, with the modified wollastonite-sericite composite material as the core and PCL as the shell.

[0023] The present invention also provides application of the core-shell type wollastonite-sericite-PCL composite material in engineering plastics.

[0024] Beneficial effects of the present invention:

[0025] The core-shell type wollastonite-sericite-PCL composite material prepared by the present invention has a core-shell structure with a modified wollastonite-sericite composite as a core and PCL as a shell. Wollastonite has high hardness and good wear resistance, and sericite has excellent sliding and impact resistance. Wollastonite and sericite are selected as core materials, which can significantly improve the rigidity and strength of the composite material, and sericite has excellent heat resistance, which can improve the thermal stability of the composite material; PCL is selected as a shell layer, which can protect the core material, reduce the impact of the external environment on the core material, and provide better impact resistance and toughness, and PCL has good melt fluidity, and the PCL shell layer can improve the processing performance of the composite material, making it easier to form and process. The wollastonite-sericite-PCL composite material combines the reinforcing effect of wollastonite and sericite with the good processing performance of PCL, and can provide excellent mechanical properties, heat resistance, chemical resistance and processing adaptability in the preparation of engineering plastics, solving some problems of existing materials.

[0026] In addition, wollastonite-sericite-PCL core-shell composite materials have many advantages such as cheap and readily available raw materials, biodegradability, environmental protection and non-toxicity, and can be used in the fields of engineering plastics preparation. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a core-shell type wollastonite-sericite-PCL composite material, comprising the following steps:

[0028] Mixing wollastonite powder, water and a first composite dispersant to obtain wollastonite powder slurry;

[0029] Mixing sericite powder, water and a second composite dispersant to obtain sericite powder slurry;

[0030] The wollastonite powder slurry, the sericite powder slurry and the slurry compounding agent are mixed for compounding, and the obtained composite slurry is sequentially dried, ground and sieved to obtain a wollastonite-sericite composite;

[0031] The wollastonite-sericite composite is mixed with a silane coupling agent and modified to obtain a modified wollastonite-sericite composite;

[0032] The modified wollastonite-sericite composite material, an organic solvent, ε-caprolactone, an initiator and a catalyst are mixed and polymerized to obtain a core-shell type wollastonite-sericite-PCL composite material.

[0033] The present invention preferably mixes wollastonite powder, water and a first composite dispersant, and performs a first grinding to obtain a wollastonite powder slurry; the wollastonite powder is preferably acicular wollastonite powder, and the particle size is preferably 400 meshes. The large mesh number of the wollastonite powder indicates that the material has a small particle size, has better dispersibility and uniformity, can effectively avoid particle aggregation, and improve the overall performance of the composite material.

[0034] In the present invention, the first composite dispersant is preferably polyethylene glycol fatty acid sodium and sodium dodecyl sulfate, and the mass of the first composite dispersant is preferably 5-9‰ of the mass of the wollastonite powder, further preferably 7-9‰, and more preferably 8-9‰; the mass ratio of the polyethylene glycol fatty acid sodium to the sodium dodecyl sulfate is preferably 1:4-1:6, further preferably 1:4-1:5, and more preferably 1:4.

[0035] In the present invention, the first grinding is preferably carried out in a first vertical stirred mill, the grinding medium used is preferably commercially available micro-spherical porous zirconia, with a Mohs hardness of 8 and a diameter of 4 to 6 mm, the stirring time is 2 h, and the grinding temperature is preferably 70 to 75°C, more preferably 70 to 73°C, and more preferably 70°C.

[0036] In the present invention, the solid content of the wollastonite powder slurry is preferably 60-65wt%, more preferably 60-63wt%, and more preferably 60wt%.

[0037] In the present invention, sericite powder, water and a second composite dispersant are preferably mixed and subjected to a second grinding to obtain sericite powder slurry; the sericite powder is preferably flaky sericite powder, and the particle size is preferably 400 meshes.

[0038] In the present invention, the second composite dispersant is preferably sodium polyacrylate and sodium stearate, and the mass of the second composite dispersant is preferably 5-9‰ of the mass of the sericite powder, further preferably 7-9‰, and more preferably 8-9‰; the mass ratio of the sodium polyacrylate to the sodium stearate is preferably 1:4-1:6, further preferably 1:4-1:5, and more preferably 1:4.

[0039] In the present invention, the second grinding is preferably carried out in a second vertical stirred mill, the grinding medium used is preferably commercially available micro-spherical porous zirconia, with a Mohs hardness of 9 and a diameter of 3 to 5 mm, the stirring time is 2 h, and the grinding temperature is preferably 80 to 85°C, more preferably 80 to 83°C, and more preferably 80°C.

[0040] In the present invention, the solid content of the sericite powder slurry is preferably 55-60wt%, more preferably 58-60wt%, and more preferably 60wt%.

[0041] The present invention preferably mixes the wollastonite powder slurry, the sericite powder slurry and a slurry compounding agent for compounding, and the obtained composite slurry is dried in an electric heated blast drying oven at 60° C. for 24 hours and then ground and sieved with a 400-mesh sieve to obtain a 400-mesh wollastonite-sericite composite.

[0042] In the present invention, the slurry compounding agent preferably includes one or more of sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4-acid, and 2-naphthylamine-1-sulfonic acid. When the slurry compounding agent is two or more of the above-mentioned types, there is no special limitation on the ratio between different types of slurry compounding agents, which can be adjusted according to actual needs; more preferably, when the slurry compounding agent is sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4-acid, and 2-naphthylamine-1-sulfonic acid, the mass ratio of sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4-acid, and 2-naphthylamine-1-sulfonic acid is preferably 2:1:1:1, and the mass of the slurry compounding agent is preferably 4-8‰ of the total mass of the wollastonite powder and the sericite powder, further preferably 5-8‰, and more preferably 6-8‰; by adding the slurry compounding agent, the surface activity of the particles in the slurry can be changed.

[0043] In the present invention, the solid content of the composite slurry is preferably 65-70wt%, more preferably 68-70wt%, and more preferably 70wt%.

[0044] In the present invention, the composite is preferably carried out in a third vertical stirred mill, and the grinding medium used is preferably commercially available micro-spherical porous zirconia with a Mohs hardness of 8 and a diameter of 4 to 5 mm; the composite is preferably carried out at room temperature, and the time is preferably 2 hours; the wollastonite powder and the sericite powder can be composited and coated by stirring in the vertical stirred mill.

[0045] The present invention preferably stirs and mixes the wollastonite-sericite composite with a silane coupling agent to perform modification to obtain a modified wollastonite-sericite composite; the silane coupling agent preferably includes one or more of γ-methacryloxypropyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane, and further preferably includes γ-methacryloxypropyltrimethoxysilane.

[0046] In the present invention, the mass ratio of the silane coupling agent to the wollastonite-sericite composite is preferably (1-2):(100-120), more preferably (1.25-2):(105-120), and more preferably (1.5-2):(110-120).

[0047] In the present invention, the modification temperature is preferably 80-90°C, more preferably 85-90°C, and more preferably 90°C; the stirring and mixing speed is preferably 80-100 r / min, more preferably 90-100 r / min, and more preferably 95-100 r / min.

[0048] The present invention preferably dissolves the modified wollastonite-sericite composite in an organic solvent for ultrasonic dispersion, then mixes with ε-caprolactone, an initiator and a catalyst, continues stirring, removes the solvent under reduced pressure, introduces argon, repeats 4 times, and conducts polymerization reaction under vacuum sealing conditions.

[0049] In the present invention, the mass ratio of the modified wollastonite-sericite composite to the ε-caprolactone is preferably (100-120):(100-200), more preferably (105-120):(125-200), and more preferably (110-120):(150-200).

[0050] In the present invention, the solvent preferably includes one of toluene and dichloromethane, and is more preferably anhydrous toluene. The mass ratio of the solvent to the ε-caprolactone monomer is preferably (150-250):(100-200).

[0051] In the present invention, the initiator preferably includes one of glycerol, sodium nitrite and aniline, and the mass ratio of the initiator to the ε-caprolactone is preferably 1:(100-200), more preferably 1:(125-200), and more preferably 1:(150-200).

[0052] In the present invention, the catalyst preferably includes one of stannous octoate and stannous chloride, and the mass ratio of the catalyst to the ε-caprolactone is preferably 0.1-0.5:(100-200), more preferably 0.2-0.5:(100-200), and more preferably 0.3-0.5:(100-200).

[0053] In the present invention, the polymerization reaction temperature is preferably 120-140° C., more preferably 130-140° C., and more preferably 135-140° C.; the polymerization reaction time is preferably 36 hours.

[0054] After the polymerization reaction is completed, the present invention preferably washes the product with anhydrous ethanol, centrifuges and dries it to obtain a core-shell wollastonite-sericite-PCL composite material.

[0055] The present invention also provides a core-shell type wollastonite-sericite-PCL composite material prepared by the above preparation method, with the modified wollastonite-sericite composite material as the core and PCL as the shell.

[0056] The present invention also provides application of the core-shell type wollastonite-sericite-PCL composite material in engineering plastics.

[0057] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0058] Example 1

[0059] Mix 400-mesh needle-shaped wollastonite powder, water and a first composite dispersant, wherein the first composite dispersant is polyethylene glycol fatty acid sodium and sodium dodecyl sulfate in a mass ratio of 1:4, and the mass of the first composite dispersant is 5‰ of the mass of the wollastonite powder, and pump into a first vertical stirred mill, and grind at a constant temperature of 70°C for 2 hours to obtain a wollastonite powder slurry with a solid content of 60wt%;

[0060] Mix 400 mesh flaky sericite powder, water and a second composite dispersant, wherein the second composite dispersant is sodium polyacrylate and sodium stearate in a mass ratio of 1:4, and the mass of the second composite dispersant is 5‰ of the mass of the sericite powder, pump it into a second vertical stirred mill, and grind it at a constant temperature of 80°C for 2h to obtain a sericite powder slurry with a solid content of 60wt%;

[0061] The ground wollastonite powder slurry and sericite powder slurry are pumped into a third vertical stirred mill, mixed with a slurry compounding agent (sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4 sulfonic acid, 2-naphthylamine-1-sulfonic acid in a mass ratio of 2:1:1:1), the mass of the slurry compounding agent is 4‰ of the total mass of the wollastonite powder and the sericite powder, water is added to prepare a composite slurry with a solid content of 70wt%, and the stirring treatment is continued for 2h. The obtained composite slurry is placed in an electric heated blast drying oven at 60°C and dried for 24h, then ground, and sieved with a 400-mesh sieve to obtain a 400-mesh wollastonite-sericite composite;

[0062] 100 parts of wollastonite-sericite composite were added to 1 part of γ-methacryloxypropyltrimethoxysilane (KH570), and the composite was modified at a speed of 80 r / min and a temperature of 80° C. to obtain a modified wollastonite-sericite composite;

[0063] 100 parts of modified wollastonite-sericite composite were dissolved in toluene solution and ultrasonically dispersed, then transferred to a 100 mL three-necked flask, 100 parts of ε-caprolactone, 1 part of propylene glycol and 0.1 g of stannous octoate were added in sequence, the mixture was stirred continuously, the solvent was removed under reduced pressure, and argon was introduced, and this process was repeated 4 times. The solution in the three-necked flask was placed at 120° C. for reaction for 36 h. After the reaction was completed, the product was washed with anhydrous ethanol, centrifuged and dried to obtain the core-shell wollastonite-sericite-PCL composite material of Example 1.

[0064] Embodiment 2:

[0065] Mix 400-mesh needle-shaped wollastonite powder, water and a first composite dispersant, wherein the first composite dispersant is polyethylene glycol fatty acid sodium and sodium dodecyl sulfate in a mass ratio of 1:4, and the mass of the first composite dispersant is 6‰ of the mass of the wollastonite powder, and pump into a first vertical stirred mill, and grind at a constant temperature of 70°C for 2 hours to obtain a wollastonite powder slurry with a solid content of 60wt%;

[0066] Mix 400 mesh flaky sericite powder, water and a second composite dispersant, wherein the second composite dispersant is sodium polyacrylate and sodium stearate in a mass ratio of 1:4, and the mass of the second composite dispersant is 6‰ of the mass of the sericite powder, and pump into a second vertical stirred mill, and grind at a constant temperature of 80°C for 2h to obtain a sericite powder slurry with a solid content of 60wt%;

[0067] The ground wollastonite powder slurry and sericite powder slurry are pumped into a third vertical stirred mill, mixed with a slurry compounding agent (sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4 sulfonic acid, 2-naphthylamine-1-sulfonic acid in a mass ratio of 2:1:1:1), the mass of the slurry compounding agent is 5‰ of the total mass of the wollastonite powder and the sericite powder, water is added to prepare a composite slurry with a solid content of 70wt%, and the stirring treatment is continued for 2h. The obtained composite slurry is placed in an electric heated blast drying oven at 60°C and dried for 24h, then ground, and sieved with a 400-mesh sieve to obtain a 400-mesh wollastonite-sericite composite;

[0068] 105 parts of wollastonite-sericite composite were added to 1.25 parts of γ-methacryloxypropyltrimethoxysilane (KH570), and the mixture was modified at a speed of 80 r / min and a temperature of 90° C. to obtain a modified wollastonite-sericite composite powder;

[0069] 105 parts of modified wollastonite-sericite composite were dissolved in toluene solution and ultrasonically dispersed, then transferred to a 100 mL three-necked flask, 125 parts of ε-caprolactone, 1 part of propylene glycol and 0.2 g of stannous octoate were added in sequence, the mixture was stirred continuously, the solvent was removed under reduced pressure, and argon was introduced, and this process was repeated 4 times. The solution in the three-necked flask was placed at 120° C. for reaction for 36 hours. After the reaction was completed, the product was washed with anhydrous ethanol, centrifuged and dried to obtain the core-shell wollastonite-sericite-PCL composite material of Example 2.

[0070] Embodiment 3:

[0071] Mix 400-mesh needle-shaped wollastonite powder, water and a first composite dispersant, wherein the first composite dispersant is polyethylene glycol fatty acid sodium and sodium dodecyl sulfate in a mass ratio of 1:4, and the mass of the first composite dispersant is 7‰ of the mass of the wollastonite powder, and pump into a first vertical stirred mill, and grind at a constant temperature of 70°C for 2 hours to obtain a wollastonite powder slurry with a solid content of 60wt%;

[0072] Mix 400 mesh flaky sericite powder, water and a second composite dispersant, wherein the second composite dispersant is sodium polyacrylate and sodium stearate in a mass ratio of 1:4, and the mass of the second composite dispersant is 7‰ of the mass of the sericite powder, and pump into a second vertical stirred mill, and grind at a constant temperature of 80°C for 2h to obtain a sericite powder slurry with a solid content of 60wt%;

[0073] The ground wollastonite powder slurry and sericite powder slurry are pumped into a third vertical stirred mill, mixed with a slurry compounding agent (sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4 sulfonic acid, 2-naphthylamine-1-sulfonic acid in a mass ratio of 2:1:1:1), the mass of the slurry compounding agent is 6‰ of the total mass of the wollastonite powder and the sericite powder, water is added to prepare a composite slurry with a solid content of 70wt%, and the stirring treatment is continued for 2h. The obtained composite slurry is placed in an electric heated blast drying oven at 60°C and dried for 24h, then ground, and sieved with a 400-mesh sieve to obtain a 400-mesh wollastonite-sericite composite;

[0074] 110 parts of wollastonite-sericite composite was added to 1.5 parts of γ-methacryloxypropyltrimethoxysilane (KH570), and the composite was modified at a speed of 90 r / min and a temperature of 90° C. to obtain a modified wollastonite-sericite composite;

[0075] 110 parts of modified wollastonite-sericite composite were dissolved in toluene solution and ultrasonically dispersed, then transferred to a 100 mL three-necked flask, 150 parts of ε-caprolactone, 1 part of propylene glycol and 0.3 g of stannous octoate were added in sequence, the mixture was stirred continuously, the solvent was removed under reduced pressure, and argon was introduced, and this process was repeated 4 times. The solution in the three-necked flask was placed at 130° C. for reaction for 36 hours. After the reaction was completed, the product was washed with anhydrous ethanol, centrifuged and dried to obtain the core-shell wollastonite-sericite-PCL composite material of Example 3.

[0076] Embodiment 4:

[0077] Mix 400-mesh needle-shaped wollastonite powder, water and a first composite dispersant, wherein the first composite dispersant is polyethylene glycol fatty acid sodium and sodium dodecyl sulfate in a mass ratio of 1:4, and the mass of the first composite dispersant is 8‰ of the mass of the wollastonite powder, and pump into a first vertical stirred mill, and grind at a constant temperature of 70°C for 2 hours to obtain a wollastonite powder slurry with a solid content of 60wt%;

[0078] Mix 400 mesh flaky sericite powder, water and a second composite dispersant, wherein the second composite dispersant is sodium polyacrylate and sodium stearate in a mass ratio of 1:4, and the mass of the second composite dispersant is 8‰ of the mass of the sericite powder, pump it into a second vertical stirred mill, and grind it at a constant temperature of 80°C for 2h to obtain a sericite powder slurry with a solid content of 60wt%;

[0079] The ground wollastonite powder slurry and sericite powder slurry are pumped into a third vertical stirred mill, mixed with a slurry compounding agent (sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4 sulfonic acid, 2-naphthylamine-1-sulfonic acid in a mass ratio of 2:1:1:1), the mass of the slurry compounding agent is 7‰ of the total mass of the wollastonite powder and the sericite powder, water is added to prepare a composite slurry with a solid content of 70wt%, and the stirring treatment is continued for 2h. The obtained composite slurry is placed in an electric heated blast drying oven at 60°C and dried for 24h, then ground, and sieved with a 400-mesh sieve to obtain a 400-mesh wollastonite-sericite composite;

[0080] 115 parts of wollastonite-sericite composite was added to 1.75 parts of γ-methacryloxypropyltrimethoxysilane (KH570), and the composite was modified at a speed of 90 r / min and a temperature of 90° C. to obtain a modified wollastonite-sericite composite;

[0081] 115 parts of modified wollastonite-sericite composite were added to toluene solution for ultrasonic dispersion, and then transferred to a 100 mL three-necked flask. 175 parts of ε-caprolactone, 1 part of propylene glycol and 0.4 g of stannous octoate were added in sequence. The mixture was stirred continuously, and the solvent was removed under reduced pressure. Argon was then introduced, and this process was repeated 4 times. The solution in the three-necked flask was placed at 130° C. for reaction for 36 hours. After the reaction was completed, the product was washed with anhydrous ethanol, and the core-shell wollastonite-sericite-PCL composite material of Example 4 was obtained by centrifugation and drying.

[0082] Embodiment 5:

[0083] Mix 400-mesh needle-shaped wollastonite powder, water and a first composite dispersant, wherein the first composite dispersant is polyethylene glycol fatty acid sodium and sodium dodecyl sulfate in a mass ratio of 1:4, and the mass of the first composite dispersant is 9‰ of the mass of the wollastonite powder, and pump into a first vertical stirred mill, and grind at a constant temperature of 70°C for 2 hours to obtain a wollastonite powder slurry with a solid content of 60wt%;

[0084] Mix 400 mesh flaky sericite powder, water and a second composite dispersant, wherein the second composite dispersant is sodium polyacrylate and sodium stearate in a mass ratio of 1:4, and the mass of the second composite dispersant is 9‰ of the mass of the sericite powder, and pump into a second vertical stirred mill, and grind at a constant temperature of 80°C for 2h to obtain a sericite powder slurry with a solid content of 60wt%;

[0085] The ground wollastonite powder slurry and sericite powder slurry are pumped into a third vertical stirred mill, mixed with a slurry compounding agent (sodium lignin sulfonate, sodium trifluoromethylsulfinate, 4-aminoazobenzene-4 sulfonic acid, 2-naphthylamine-1-sulfonic acid in a mass ratio of 2:1:1:1), the mass of the slurry compounding agent is 8‰ of the total mass of the wollastonite powder and the sericite powder, water is added to prepare a composite slurry with a solid content of 70wt%, and the stirring treatment is continued for 2h. The obtained composite slurry is placed in an electric heated blast drying oven at 60°C and dried for 24h, then ground, and sieved with a 400-mesh sieve to obtain a 400-mesh wollastonite-sericite composite;

[0086] 120 parts of wollastonite-sericite composite were added to 2 parts of γ-methacryloxypropyltrimethoxysilane (KH570), and the composite was modified at a speed of 100 r / min and a temperature of 90° C. to obtain a modified wollastonite-sericite composite;

[0087] 120 parts of modified wollastonite-sericite composite were dissolved in toluene solution and ultrasonically dispersed, then transferred to a 100 mL three-necked flask, 200 parts of ε-caprolactone, 1 part of propylene glycol and 0.5 g of stannous octoate were added in sequence, the mixture was stirred continuously, the solvent was removed under reduced pressure, and argon was introduced, and this process was repeated 4 times. The solution in the three-necked flask was placed at 140° C. for reaction for 36 hours. After the reaction was completed, the product was washed with anhydrous ethanol, centrifuged and dried to obtain the core-shell wollastonite-sericite-PCL composite material of Example 5.

[0088] Performance Testing

[0089] The wollastonite-sericite-PCL composite materials obtained in Examples 1 to 5 were tested for impact strength, tensile strength and elongation at break:

[0090] Impact strength: tested in accordance with GB / T1843-2008 standard;

[0091] Tensile strength: tested in accordance with GB / T1040-2006 standard;

[0092] Elongation at break: Tested in accordance with GB / T1040-2006 standard;

[0093] The performance test results of the wollastonite-sericite-PCL composite materials of Examples 1 to 5 are shown in Table 1.

[0094] Table 1 Performance test results of wollastonite-sericite-PCL composite materials of Examples 1 to 5

[0095] <![CDATA[Impact strength (KJ / m 2 )]]> Tensile strength(MPa) Elongation at break (%) Example 1 25.7 18.25 69.53 Example 2 28.3 20.36 72.36 Example 3 29.5 24.72 86.71 Example 4 30.5 25.94 88.42 Example 5 32.6 26.31 92.34

[0096] It can be seen from Examples 1 to 5 that the present invention provides a method for preparing a core-shell wollastonite-sericite-PCL composite material. The obtained core-shell wollastonite-sericite-PCL composite material has a modified wollastonite-sericite composite as the core, a layer of polycaprolactone is coated on the outside of the core, and the compatibility of the two is improved by using a silane coupling agent. The obtained composite material has excellent mechanical properties, and the raw materials are cheap and the preparation method is simple, which greatly broadens the application field of polycaprolactone.

[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a core-shell wollastonite-sericite-PCL composite material, characterized in that: The following steps are involved: Mixing wollastonite powder, water and a first composite dispersant to obtain wollastonite powder slurry; Mixing sericite powder, water and a second composite dispersant to obtain sericite powder slurry; The wollastonite powder slurry, the sericite powder slurry and the slurry compounding agent are mixed for compounding, and the obtained composite slurry is sequentially dried, ground and sieved to obtain a wollastonite-sericite composite; The wollastonite-sericite composite is mixed with a silane coupling agent and modified to obtain a modified wollastonite-sericite composite; The modified wollastonite-sericite composite material, an organic solvent, ε-caprolactone, an initiator and a catalyst are mixed and polymerized to obtain a core-shell type wollastonite-sericite-PCL composite material.

2. The preparation method according to claim 1, characterized in that: The first composite dispersant is polyethylene glycol fatty acid sodium and sodium dodecyl sulfate, the mass of the first composite dispersant is 5-9‰ of the mass of the wollastonite powder, and the mass ratio of the polyethylene glycol fatty acid sodium to the sodium dodecyl sulfate is 1:4-1:6; The second composite dispersant is sodium polyacrylate and sodium stearate, the mass of the second composite dispersant is 5-9‰ of the mass of the sericite powder, and the mass ratio of the sodium polyacrylate to the sodium stearate is 1:4-1:

6.

3. The preparation method according to claim 1, characterized in that: The solid content of the wollastonite powder slurry is 60-65wt%, the solid content of the sericite powder slurry is 55-60wt%, and the solid content of the composite slurry is 65-70wt%.

4. The preparation method according to claim 1, characterized in that: The slurry compounding agent includes one or more of sodium lignin sulfonate, sodium trifluoromethanesulfinate, 4-aminoazobenzene-4-acid, and 2-naphthylamine-1-sulfonic acid. The mass of the slurry compounding agent is 4 to 8‰ of the total mass of the wollastonite powder and the sericite powder.

5. The preparation method according to claim 1, characterized in that: The silane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane, and the mass ratio of the silane coupling agent to the wollastonite-sericite composite is (1-2):(100-120).

6. The preparation method according to claim 1, characterized in that: The modification temperature is 80-90° C., and the stirring speed is 80-100 r / min.

7. The preparation method according to claim 1, characterized in that: The mass ratio of the modified wollastonite-sericite composite to the ε-caprolactone is (100-120):(100-200).

8. The preparation method according to claim 1, characterized in that: The solvent includes one of toluene and dichloromethane; the initiator includes one of propylene glycol, sodium nitrite and aniline, and the mass ratio of the initiator to the ε-caprolactone is 1:(100-200); the catalyst includes one of stannous octoate and stannous chloride, and the mass ratio of the catalyst to the ε-caprolactone is (0.1-0.5):(100-200).

9. The core-shell wollastonite-sericite-PCL composite material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The modified wollastonite-sericite composite was used as the core and PCL as the shell.

10. Use of the core-shell wollastonite-sericite-PCL composite material according to claim 9 in engineering plastics.

Citation Information

Cited By

  • Flame-retardant PET (Polyethylene Terephthalate) composite label material

    CN122080478A