Method for efficiently preparing hierarchical pore MIL-100 (Fe) at room temperature

By using solution preparation and gentle reaction conditions at room temperature, the problems of high temperature, high pressure and multi-stage pore control in traditional methods are solved, and the multi-stage pore MIL-100 (Fe) is achieved with low energy consumption and efficient preparation of multi-stage pore MIL-100 (Fe). Excellent material performance and suitable for industrial applications.

CN118909269APending Publication Date: 2024-11-08NANTONG INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411043612.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The traditional MIL-100 (Fe) preparation method requires high temperature and high pressure conditions, which limits its large-scale production and industrial applications, and is difficult to achieve efficient synthesis at room temperature, especially fine regulation of multi-stage pore structures.

Method used

MIL-100 (Fe) was prepared at room temperature using the steps of solution preparation, mixing and stirring, separation and washing, drying and activation. Using ethanol/N,N dimethylformamide mixed solvent and hydrated iron salt, ammonium fluoride was added to form a poly The stage pore structure reduces energy consumption and pollution through mild reaction conditions.

Benefits of technology

It has achieved low energy consumption, low pollution and efficient preparation of multi-stage pore MIL-100 (Fe), excellent material performance, a specific surface area of ​​1047m2/g and a multi-stage pore structure, which is suitable for gas adsorption and separation applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909269A_ABST
    Figure CN118909269A_ABST
Patent Text Reader

Abstract

The invention discloses a method for efficiently preparing hierarchical pore MIL-100 (Fe) at room temperature, the prepared MIL-100 (Fe) has a hierarchical pore structure, and the method comprises the following steps: dissolving 1, 3, 5-trimesic acid in an ethanol / N, N-dimethylformamide mixed solvent to prepare a solution a; fe (NO3) 3.9 H2O is dissolved in water, a certain amount of ammonium fluoride is added, and orange gel b is prepared; mixing the solution a and the orange gel b at room temperature, and stirring for a certain time to form gel c; the preparation method comprises the following steps: carrying out solid-liquid separation through centrifugation, washing a solid obtained by separation with distilled water and ethanol at room temperature, soaking in dichloromethane, drying a soaked product for a period of time in an environment of 70 DEG C, and activating for a period of time in an environment of 150 DEG C to prepare orange powder d which is F-MIL-100 (Fe). According to the method disclosed by the invention, the hierarchical pore MIL-100 (Fe) is prepared with low energy consumption, low pollution and high yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of metal organic framework materials, in particular to a method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature. Background Art

[0002] MIL-100(Fe), as a metal-organic framework (MOF) material with iron as the central ion and phthalic acid as the organic ligand, has broad application prospects in gas adsorption and separation, catalytic reactions and many other fields. Traditional preparation methods of MIL-100(Fe) mainly include solvothermal method and template method, but these methods usually require high temperature and high pressure conditions and long reaction time. Moreover, traditional preparation methods can rarely achieve efficient synthesis at room temperature, which limits the large-scale production and industrial application of MIL-100(Fe). In addition, the fine control of pore structure is also one of the challenges faced by traditional methods, especially the preparation of MIL-100(Fe) with a multi-level pore structure, which is crucial to improving the gas adsorption and separation performance of the material. Summary of the invention

[0003] Purpose of the invention: In order to overcome the deficiencies in the prior art, the present invention provides a method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature, thereby achieving low energy consumption, low pollution and high yield in the preparation of multi-level porous MIL-100 (Fe).

[0004] Technical solution: To achieve the above purpose, the present invention provides a method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature, wherein the prepared MIL-100 (Fe) has a multi-level porous structure, and specifically comprises the following steps:

[0005] Step I, solution preparation, dissolving 1,3,5-trimethylbenzene trimesic acid in an ethanol / N,N-dimethylformamide mixed solvent to obtain solution a; dissolving hydrated iron salt in water, and adding a certain amount of ammonium fluoride to obtain gel b;

[0006] Step II, mixing and stirring, mixing the solution a and the gel b at 25-35° C., and stirring for a certain period of time to form a gel c;

[0007] Step III, separation and washing, solid-liquid separation is achieved by centrifugation, the separated solid is washed with distilled water and ethanol at 25-35°C, and then soaked in dichloromethane;

[0008] Step IV, drying and activation, the soaked product is first dried at 70°C for a period of time, and then activated at 150°C for a period of time to obtain powder d, wherein the powder d is F-MIL-100 (Fe).

[0009] Furthermore, in step I, 5%-15% of ammonium fluoride is added.

[0010] Furthermore, in step I, in the ethanol / N,N-dimethylformamide mixed solvent, the mixing ratio of ethanol to N,N-dimethylformamide is 1:1.

[0011] Furthermore, the concentration of 1,3,5-trimethylbenzenecarboxylic acid in the solution a is 0.01-0.1 g / ml.

[0012] Furthermore, the concentration of Fe(NO3)3·9H2O in the gel b is 0.05-0.5 g / ml.

[0013] Furthermore, the mixing volume ratio of the solution a and the gel b is 1:1 to 5:1.

[0014] Furthermore, the stirring time for the formation of the gel c is 72 hours, the washing time of the solid product after centrifugal separation is 1 hour, the drying time is 24 hours, and the activation time is 24 hours.

[0015] Furthermore, the solid product obtained by centrifugal separation is washed and then soaked in the dichloromethane twice, each time for 24-48 hours.

[0016] Beneficial effects: The method of the present invention provides a method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature, which adopts milder reaction conditions to synthesize MIL-100 (Fe), does not require high temperature and high pressure conditions, reduces equipment requirements and energy consumption; shortens the preparation cycle, improves production efficiency; reduces the amount of DMF used, and reduces pollution to the environment; the prepared MIL-100 (Fe) has a multi-level porous structure and excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is the nitrogen adsorption isotherm of 5% F-MIL-100 (Fe) of the present invention;

[0018] Figure 2 This is the nitrogen adsorption isotherm of 10% F-MIL-100(Fe) of the present invention. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with the accompanying drawings.

[0020] like Figure 1-2 The method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature, wherein the prepared MIL-100 (Fe) has a multi-level porous structure, specifically comprises the following steps:

[0021] Step I, solution preparation, dissolving 1,3,5-trimethylbenzene trimesic acid in an ethanol / N,N-dimethylformamide mixed solvent to obtain solution a; dissolving hydrated iron salt in water, and adding 5%-15% ammonium fluoride to obtain gel b.

[0022] Step II: Mixing and stirring: mixing the solution a and the gel b at 25-35° C. and stirring for a certain period of time to form a gel c.

[0023] Step III, separation and washing, solid-liquid separation is achieved by centrifugation, the separated solid is washed with distilled water and ethanol at 25-35°C, and then soaked in dichloromethane.

[0024] Step IV, drying and activation, the soaked product is first dried at 70°C for a period of time, and then activated at 150°C for a period of time to obtain powder d, and the powder d is marked as 5%-15% F-MIL-100 (Fe).

[0025] Among them, the use of hydrated iron salts is conducive to the formation of high-quality MOF crystals. Hydrated iron salts slow down the deprotonation of carboxylates and delay the binding of ligands to metal centers, thereby promoting the growth of larger crystals and reducing the formation of amorphous products and impurity products. One or more water molecules can exist as ligands and form part of the three-dimensional network structure of MOF. One or more water molecules dissociate and can form protonated H3O with other water molecules. + Species and coordinated OH - Ligand; preferably, the hydrated iron salt is Fe(NO3)3·9H2O.

[0026] When ferric nitrate is dissolved in water, it is hydrolyzed to form ferric hydroxide gel. When reacting with aqueous ammonium fluoride solution, the gel part of freshly precipitated iron hydroxide (III) is converted into triammonium hexafluoroferrate (III), thereby forming a mixture of iron hydroxide and triammonium hexafluoroferrate (III), which is an orange gel b.

[0027] The generated triammonium hexafluoroferrate (III) is more likely to react with the ligand to generate MIL-100(Fe), which is beneficial to the room temperature synthesis of MIL-100(Fe).

[0028] The ethanol / N, N-dimethylformamide mixed solvent is used as the solvent of the organic ligand. First, the mixed solvent provides a better dissolution environment, which is conducive to the complete dissolution of 1,3,5-trimethylbenzene, thereby ensuring the smooth progress of the synthesis reaction. In addition, ethanol and DMF have good mutual solubility. After mixing, they can provide a more uniform reaction environment, which is conducive to the uniform dispersion and effective assembly of metal ions and organic ligands. And using ethanol as part of the mixed solvent and washing with ethanol after the synthesis is completed can more effectively remove unreacted raw materials and by-products; and then soaking in dichloromethane, due to the low boiling point of dichloromethane, it is easier to replace the DMF in the pores of the MOF material, thereby simplifying the post-processing process and achieving efficient synthesis at room temperature.

[0029] In the ethanol / N,N-dimethylformamide mixed solvent, the mixing ratio of ethanol to N,N-dimethylformamide is 1:1. The 1:1 mixing ratio is the result of experimental optimization, which can balance the advantages and disadvantages of the two solvents, achieve optimal solubility, reaction rate and material properties, and help promote uniform nucleation and growth of MOF materials at room temperature, while reducing solvent volatilization and maintaining the stability of the reaction system.

[0030] The concentration of 1,3,5-trimethylbenzene in the solution a is 0.01-0.1 g / ml. The concentration of Fe(NO3)3·9H2O in the gel b is 0.05-0.5 g / ml. The mixed volume ratio of the solution a and the gel b is 1:1 to 5:1.

[0031] Preferably, the concentration of 1,3,5-trimethylbenzene in the solution a is 0.025 g / ml. The concentration of Fe(NO3)3·9H2O in the gel b is 0.1442 g / ml. The mixed volume ratio of the solution a and the gel b is 2:1.

[0032] Preferably, the stirring time for the formation of the gel c is 72 hours, the washing time of the solid product after centrifugal separation is 1 hour, the drying time is 24 hours, and the activation time is 24 hours. After washing, the solid product obtained by centrifugal separation is soaked in the dichloromethane twice, each soaking for 24-48 hours.

[0033] By adding ammonium fluoride as a structure directing agent, it is helpful to form a multi-level pore structure. Its concentration affects the distribution of pore sizes. Two specific examples are provided below:

[0034] Example 1: 0.5 g of 1,3,5-trimethylbenzene trimesic acid was dissolved in an ethanol / N,N-dimethylformamide mixed solvent to obtain a solution a1; 1.442 g of Fe(NO3)3·9H2O was dissolved in 10 ml of water, and 25 mg of ammonium fluoride was added to obtain an orange gel b1; the solution a1 and the orange gel b1 were mixed at room temperature to form a gel c1, and stirred for 72 hours; the separated solid was washed with distilled water and ethanol for 1 hour at room temperature by centrifugation, and then immersed in dichloromethane twice; the immersed product was first dried at 70°C for 24 hours, and then activated at 150°C for 24 hours to obtain an orange powder d1, and the orange powder d1 was marked as 5% F-MIL-100 (Fe).

[0035] like Figure 1 As shown in the figure, the nitrogen adsorption isotherm of 5% F-MIL-100 (Fe) shows the characteristics of a typical IV type adsorption isotherm, indicating that the prepared material is a multi-level porous material with a specific surface area of ​​1047m 2 / g, which is comparable to the materials prepared by traditional methods. Between the relative pressure of 0-0.1, the adsorption isotherm has a significant increase, indicating the existence of microporous structure. Between the medium pressure section of 0.4-0.7, there is an obvious hysteresis loop, indicating the existence of mesopores. The pore size distribution diagram further confirms the existence of mesopores. It can be seen from the figure that the material has a significant pore size distribution at 3.6nm.

[0036] Example 2: Compared with Example 1, the input amount of ammonium fluoride was changed to 50 mg, and other conditions remained unchanged. Finally, an orange powder d2 was obtained, which was marked as 10% F-MIL-100 (Fe).

[0037] like Figure 2 As shown in the figure, the nitrogen adsorption isotherm of 10% F-MIL-100 (Fe) also shows the characteristics of a typical IV type adsorption isotherm, indicating that the prepared material is still a multi-level porous material. Between the relative pressure of 0-0.1, the adsorption isotherm has a significant increase, indicating the existence of a microporous structure. Between the medium pressure section of 0.3-0.6, the adsorption isotherm has an obvious hysteresis loop, indicating the existence of mesopores. The pore size distribution diagram further confirms the existence of mesopores. It can be seen from the figure that the material has an obvious pore size distribution at 3.5nm.

[0038] After many groups of experiments, it was found that when the input amount of ammonium fluoride was controlled at 5%-15%, multi-level pore-MIL-100(Fe) could be obtained. By comparing the results of the above two embodiments, it can be seen that the optimal value of the ammonium fluoride content is 5%. As the ammonium fluoride content increases, the mesopore pore size distribution size will decrease. This is because when the ammonium fluoride content is high, the excess F element will coordinate with the F in MOF, resulting in changes in the local structure of MOFs, thereby changing the pore size distribution. In addition, iron fluoride by-products will be generated, resulting in a decrease in specific surface area.

[0039] In summary, the method of the present invention can achieve efficient preparation of multi-level porous MIL-100 (Fe) at room temperature, and the optimal product is 5% F-MIL-100 (Fe).

[0040] The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the above principles of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature, characterized in that: The prepared MIL-100(Fe) has a multi-level pore structure, which specifically includes the following steps: Step I, solution preparation, dissolving 1,3,5-trimethylbenzene trimesic acid in an ethanol / N,N-dimethylformamide mixed solvent to obtain solution a; dissolving hydrated iron salt in water, and adding a certain amount of ammonium fluoride to obtain gel b; Step II, mixing and stirring, mixing the solution a and the gel b at 25-35° C., and stirring for a certain period of time to form a gel c; Step III, separation and washing, solid-liquid separation is achieved by centrifugation, the separated solid is washed with distilled water and ethanol at 25-35°C, and then soaked in dichloromethane; Step IV, drying and activation, the soaked product is first dried at 70°C for a period of time, and then activated at 150°C for a period of time to obtain powder d, wherein the powder d is F-MIL-100 (Fe).

2. The method for efficiently preparing multi-level porous MIL-100(Fe) at room temperature according to claim 1, characterized in that: In step I, 5%-15% of ammonium fluoride is added.

3. The method for efficiently preparing multi-level porous MIL-100(Fe) at room temperature according to claim 2, characterized in that: In step I, in the ethanol / N,N-dimethylformamide mixed solvent, the mixing ratio of ethanol to N,N-dimethylformamide is 1:

1.

4. The method for efficiently preparing multi-level porous MIL-100(Fe) at room temperature according to claim 3, characterized in that: The concentration of 1,3,5-trimethylbenzenecarboxylic acid in the solution a is 0.01-0.1 g / ml.

5. The method for efficiently preparing multi-level porous MIL-100(Fe) at room temperature according to claim 4, characterized in that: The concentration of Fe(NO3)3·9H2O in the gel b is 0.05-0.5 g / ml.

6. The method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature according to claim 5, characterized in that: The mixing volume ratio of the solution a and the gel b is 1:1 to 5:

1.

7. The method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature according to claim 6, characterized in that: The stirring time for the formation of the gel c is 72 hours, the washing time of the solid product after centrifugal separation is 1 hour, the drying time is 24 hours, and the activation time is 24 hours.

8. The method for efficiently preparing multi-level porous MIL-100 (Fe) at room temperature according to claim 7, characterized in that: The solid product obtained by centrifugation is washed and then soaked in the dichloromethane twice, each time for 24-48 hours.

Citation Information

Patent Citations

  • A process for the production of titanium dioxide using aqueous fluoride

    CN101111456A

  • Preparation method of metal organic framework material MIL-100 (Fe)

    CN103242374A

  • MOPs bi-ligand adsorbing material Fe-btc(dobdc) and preparation method thereof

    CN105771907A

  • MOFs dual-metal adsorption material (Fe, Co)-BTC and preparation method thereof

    CN106076242A