Fiber-reinforced polypropylene composite material and preparation method thereof

By combining homopolymer polypropylene resin, block copolymer polypropylene resin and polyamide resin, along with compatibilizers, nucleating agents, coupling agents and antioxidants, fiber-reinforced polypropylene composites were prepared. This solved the problems of mechanical properties and thermal stability of polypropylene resin under special environments, and achieved high impact strength, tensile properties and thermal stability of the material.

CN118909352APending Publication Date: 2024-11-08ZHONGFU SHENYING CARBON FIBER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125153.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Polypropylene resin has limited mechanical properties and thermal stability under special environments, which restricts its application.

Method used

Fiber-reinforced polypropylene composites were prepared by combining homopolymer polypropylene resin, block copolymer polypropylene resin and polyamide resin, and adding compatibilizers, nucleating agents, coupling agents and antioxidants, through mixing and granulation processes.

Benefits of technology

It improves the impact strength, tensile properties and thermal stability of composite materials, while reducing material costs and expanding the range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909352A_ABST
    Figure CN118909352A_ABST
Patent Text Reader

Abstract

The invention provides a fiber-reinforced polypropylene composite material and a preparation method thereof, and relates to the technical field of composite materials. The fiber-reinforced polypropylene composite material comprises: 80-120 parts by weight of a resin matrix; 15-45 parts by weight of reinforcing fibers; 2-15 parts by weight of an auxiliary agent; the resin matrix comprises polypropylene resin and polyamide resin, and the polypropylene resin comprises homo-polypropylene resin and block co-polypropylene resin. The fiber reinforced polypropylene composite material provided by the invention has excellent tensile property, impact resistance and thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and in particular to a fiber-reinforced polypropylene composite material and a preparation method thereof. Background Art

[0002] With the continuous development of modern engineering technology, composite materials, as a new type of material, are increasingly widely used in various fields. Composite materials have the advantages of low density, high strength, and corrosion resistance, and are widely used in aerospace, automobile manufacturing, construction engineering and other fields. Among them, fiber reinforced composite materials (Fiber Reinforced Polymer, FRP) are made of carbon fiber, glass fiber, polymer fiber, metal fiber and other reinforcing materials, and are compounded with polymer matrix materials such as resin. It has the characteristics of high specific strength, large specific modulus, and good durability.

[0003] As the main component of composite materials, the properties of the resin matrix have a significant impact on the properties of the composite materials. Among them, polypropylene, as a commonly used polymer matrix material, has good molding properties and mechanical properties, but in some special environments, its mechanical properties and thermal stability are limited, which limits its application in special environments. Summary of the invention

[0004] In order to solve the above technical problems, the present application aims to provide a fiber-reinforced polypropylene composite material having excellent tensile properties, impact resistance and thermal stability.

[0005] According to the first aspect of the present application, a fiber-reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0006] 80-120 parts by weight of resin matrix;

[0007] 15-45 parts by weight of reinforcing fiber;

[0008] 2-15 parts by weight of auxiliary agent;

[0009] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0010] In some embodiments of the present application, the weight ratio of the polypropylene resin to the polyamide resin is 1.20-9.00:1.

[0011] In some embodiments of the present application, the weight ratio of the homopolymer polypropylene resin to the block copolymer polypropylene resin is 1.05-1.55:1.

[0012] In some embodiments of the present application, the crystallinity of the homopolymer polypropylene resin is 43-48%; the crystallinity of the block copolymer polypropylene resin is 38-42%.

[0013] In some embodiments of the present application, the auxiliary agent includes a combination of one or more of a compatibilizer, a nucleating agent, a coupling agent, and an antioxidant.

[0014] In some embodiments of the present application, when the auxiliary agent includes a combination of the compatibilizer, the nucleating agent, the coupling agent and the antioxidant:

[0015] The compatibilizer includes polypropylene grafted with maleic anhydride;

[0016] The nucleating agent includes calcium phthaloyl beta-alaninate;

[0017] The coupling agent includes an aluminate coupling agent and a titanate coupling agent, and the weight ratio of the aluminate coupling agent to the titanate coupling agent is 1-3:1;

[0018] The antioxidant includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].

[0019] In some embodiments of the present application, when the auxiliary agent is a composition comprising the compatibilizer, the nucleating agent, the coupling agent and the antioxidant:

[0020] The weight of the compatibilizer is 2-6% of the weight of the resin matrix;

[0021] The weight of the nucleating agent is 0.08-0.20% of the weight of the polypropylene resin;

[0022] The weight of the antioxidant is 0.25-1% of the weight of the resin matrix;

[0023] The solute mass fraction of the aqueous solution of the coupling agent is 0.35-0.8 wt %.

[0024] In some embodiments of the present application, the reinforcing fibers include chopped carbon fibers, and the chopped carbon fiber monofilaments have a diameter of 2-10 μm and a length of 1-2 mm.

[0025] According to a second aspect of the present application, a method for preparing a composite material is provided. The method for preparing a composite material is used to prepare the fiber-reinforced polypropylene composite material as described above. The method comprises:

[0026] Mixing and granulating the resin matrix and the auxiliary agent under a first preset condition to obtain composite resin particles;

[0027] The composite resin particles and the reinforcing fibers are mixed and granulated under a second preset condition to obtain the fiber-reinforced polypropylene composite material.

[0028] In some embodiments of the present application, before granulating the composite resin particles and the reinforcing fibers, the preparation method further comprises:

[0029] The reinforcing fibers are obtained by mixing the aqueous solution of the coupling agent with the initial fibers under the third preset condition and drying them.

[0030] The technical solution provided by the present application may include the following beneficial effects: the present application can enhance the toughness of the material while maintaining the mechanical properties through the combination of homopolymer polypropylene resin, block copolymer polypropylene resin and polyamide resin, so as to improve the impact strength of the composite material, and can also reduce the cost of the material, improve the processing performance and expand its application range.

[0031] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0033] Figure 1 The present invention is a flow chart of a method for preparing a composite material according to an exemplary embodiment. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme of the present application will be clearly and completely described below in combination with the embodiments of the present application and the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be arbitrarily combined with each other.

[0035] The present application provides a fiber reinforced polypropylene composite material, comprising the following raw materials in parts by weight: 80-120 parts by weight of a resin matrix; 15-45 parts by weight of reinforcing fibers; and 2-15 parts by weight of an additive. The resin matrix comprises a polypropylene resin and a polyamide resin, and the polypropylene resin comprises a homopolymer polypropylene resin and a block copolymer polypropylene resin. The present application can enhance the toughness of the material while maintaining mechanical properties through the combination of the homopolymer polypropylene resin, the block copolymer polypropylene resin and the polyamide resin, so as to improve the impact strength of the composite material, and can also reduce the cost of the material, improve the processing performance, and expand its application range.

[0036] Some specific implementation modes described below are intended to facilitate those skilled in the art to understand the present embodiment, and the present embodiment is not limited to some specific implementation modes described below.

[0037] An exemplary embodiment of the present application shows a fiber-reinforced polypropylene composite material, comprising the following raw materials in parts by weight:

[0038] 80-120 parts by weight of resin matrix;

[0039] 15-45 parts by weight of reinforcing fiber;

[0040] 2-15 parts by weight of auxiliary agent;

[0041] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0042] In this embodiment, by combining homopolymerized polypropylene resin, block copolymerized polypropylene resin and polyamide resin, the toughness of the material can be enhanced while maintaining the mechanical properties, so as to improve the impact strength of the composite material, and the cost of the material can be reduced and the processing performance can be improved; the tensile properties and thermal stability of the composite material can be improved by adding reinforcing fibers, for example, the reinforcing fibers can be carbon fibers, glass fibers, aramid fibers, etc.; the mechanical properties and processing properties of the composite material can be improved by using additives. By combining the above raw materials, the composite material obtained has excellent tensile properties and thermal stability.

[0043] Exemplarily, in one embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0044] 80 parts by weight of resin matrix;

[0045] 15 parts by weight of reinforcing fiber;

[0046] 2 parts by weight of auxiliary agent;

[0047] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0048] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0049] Resin matrix 92 parts by weight;

[0050] 35 parts by weight of reinforcing fiber;

[0051] 4 parts by weight of auxiliary agent;

[0052] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0053] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0054] Resin matrix 96 parts by weight;

[0055] 42 parts by weight of reinforcing fiber;

[0056] 3 parts by weight of auxiliary agent;

[0057] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0058] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0059] 100 parts by weight of resin matrix;

[0060] 30 parts by weight of reinforcing fiber;

[0061] 8 parts by weight of auxiliary agent;

[0062] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0063] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0064] Resin matrix 106 parts by weight;

[0065] 25 parts by weight of reinforcing fiber;

[0066] 6.6 parts by weight of auxiliary agent;

[0067] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0068] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0069] Resin matrix 108 parts by weight;

[0070] 43 parts by weight of reinforcing fiber;

[0071] 7.5 parts by weight of auxiliary agent;

[0072] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0073] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0074] Resin matrix 113 parts by weight;

[0075] 39 parts by weight of reinforcing fiber;

[0076] 8.1 parts by weight of auxiliary agent;

[0077] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0078] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0079] Resin matrix 115 parts by weight;

[0080] 22 parts by weight of reinforcing fiber;

[0081] 6 parts by weight of auxiliary agent;

[0082] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0083] In another embodiment, a fiber-reinforced polypropylene composite material includes the following raw materials in parts by weight:

[0084] 120 parts by weight of resin matrix;

[0085] 45 parts by weight of reinforcing fiber;

[0086] 15 parts by weight of auxiliary agent;

[0087] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0088] In an exemplary embodiment, the weight ratio of the polypropylene resin to the polyamide resin is 1.20-9.00:1.

[0089] Polypropylene resin, as a general-purpose plastic, has high tensile strength, compressive strength and hardness, as well as good bending fatigue resistance and heat resistance, but its impact resistance at low temperature is poor. Polyamide resin, as an engineering plastic with excellent performance, has high tensile strength, compressive strength, toughness, impact resistance and heat resistance. By compounding polypropylene resin with polyamide resin, and controlling the weight ratio of polypropylene resin to polyamide resin to 1.20-9.00:1, the resin matrix thus obtained has excellent mechanical properties and thermal stability. Wherein, polyamide can select polyamide 6 (PA6), for example, selected from polyamide resin with model M2800. Exemplarily, the weight ratio of polypropylene resin to polyamide resin can be 1.20:1, 2.52:1, 4.64:1, 6.86:1, 7.48:1, 9.00:1.

[0090] In an exemplary embodiment, the weight ratio of the homopolymer polypropylene resin to the block copolymer polypropylene resin is 1.05-1.55:1.

[0091] According to the monomer type and polymerization method used in the polymerization process of polypropylene resin, it can be divided into homopolymer polypropylene resin (PP-H), block copolymer polypropylene resin (PP-B) and random (random) copolymer polypropylene resin (PP-R). Among them, PP-H is polymerized by a single propylene monomer, which usually has high crystallinity, which makes it have good hardness, strength and heat resistance. PP-B is randomly block copolymerized by propylene and a small amount of other monomers (such as ethylene). Compared with PP-H, PP-B has better toughness and impact resistance. By compounding PP-H and PP-B, and controlling the weight ratio of the two to 1.05-1.55:1, the resin matrix can have good hardness, strength, heat resistance, toughness and impact resistance. Exemplarily, the weight ratio of homopolymer polypropylene resin to block copolymer polypropylene resin is 1.05:1, 1.24:1, 1.36:1, 1.55:1.

[0092] In an exemplary embodiment, the homopolymer polypropylene resin has a crystallinity of 43-48%; and the block copolymer polypropylene resin has a crystallinity of 38-42%.

[0093] In this embodiment, the crystallinity of the homopolymer polypropylene resin may be, for example, 43%, 45% or 48%; the crystallinity of the block copolymer polypropylene resin may be, for example, 38%, 40% or 42%. For example, the crystallinity of the homopolymer polypropylene resin is 45%, and the model is T012; the crystallinity of the block copolymer polypropylene resin is 40%, and the model is K8303.

[0094] In an exemplary embodiment, the auxiliary agent includes a combination of one or more of a compatibilizer, a nucleating agent, a coupling agent, and an antioxidant.

[0095] The compatibilizer can improve the compatibility between polypropylene resin and polyamide resin to improve the dispersibility and interfacial bonding force of the resin matrix mixture, thereby improving the physical properties and stability of the resin matrix.

[0096] Nucleating agents can promote the crystallization of polypropylene resin to improve the rigidity of the material. The combination of nucleating agents and reinforcing fibers can promote the material to form a uniform dispersion, effectively prevent crack propagation, and cooperate with reinforcing fibers to improve the tensile properties and thermal stability of the composite material.

[0097] Coupling agents can improve the interfacial bonding between reinforcing fibers and resin matrix to improve the mechanical properties and thermal stability of composite materials.

[0098] Antioxidants can improve the antioxidant properties of composite materials, reduce the degradation of composite materials caused by oxidation, and help extend the service life of composite materials.

[0099] In this embodiment, the auxiliary agent can be selected from a combination of one or more of a compatibilizer, a nucleating agent, a coupling agent, and an antioxidant. The combination of the above auxiliary agents is beneficial to improving the comprehensive properties of the composite material, such as mechanical properties, heat resistance, processing properties, and service life.

[0100] In an exemplary embodiment, when the auxiliary agent is a composition including a compatibilizer, a nucleating agent, a coupling agent and an antioxidant:

[0101] The compatibilizer includes polypropylene grafted with maleic anhydride;

[0102] Nucleating agents include calcium phthaloyl beta-alaninate;

[0103] The coupling agent includes an aluminate coupling agent and a titanate coupling agent, and the weight ratio of the aluminate coupling agent to the titanate coupling agent is 1-3;

[0104] Antioxidants include pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].

[0105] In this embodiment, the compatibilizer can be polypropylene grafted maleic anhydride (PP-g-MAH), which is a material that introduces maleic anhydride monomer into a polypropylene matrix through a grafting reaction, which can improve the compatibility, mechanical properties and heat resistance of polypropylene resin and polyamide resin, improve the fluidity of the resin matrix, and improve its processing performance. For example, the compatibilizer can be selected from polypropylene grafted maleic anhydride 1010 or 1020.

[0106] The nucleating agent can be a β-nucleating agent, whose main component is calcium phthaloyl β-alanine, which can increase the crystallinity of the polypropylene resin to improve its mechanical and thermal properties; and can also refine the grain structure of the polypropylene resin to improve the transparency, surface gloss, tensile strength, impact resistance, heat resistance, etc. of the product.

[0107] The coupling agent can be compounded by a titanate coupling agent and an aluminate coupling agent. The reinforcing fiber treated by the compounded coupling agent has good bonding strength with the resin matrix, which can reduce the peeling or cracking phenomenon that may occur during the use of the composite material, and improve the reliability and durability of the material. Among them, the titanate coupling agent can be selected from KR-TTS, UP-133, etc.; the aluminate coupling agent can be selected from SG-Al821, DL-411, etc. For example, the weight ratio of the aluminate coupling agent to the titanate coupling agent is 1:1, 2:1 or 3:1.

[0108] The antioxidant can be pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (antioxidant 1010). Antioxidant 1010 is a phenolic antioxidant with low volatility, high thermal stability, long lasting effect, and excellent antioxidant performance for polypropylene resin.

[0109] In an exemplary embodiment, when the auxiliary agent includes a combination of a compatibilizer, a nucleating agent, a coupling agent and an antioxidant:

[0110] The weight of the compatibilizer is 2-6% of the weight of the resin matrix;

[0111] The weight of the nucleating agent is 0.08-0.20% of the weight of the polypropylene resin;

[0112] The weight of the antioxidant is 0.25-1% of the weight of the resin matrix;

[0113] The solute mass fraction of the coupling agent aqueous solution is 0.35-0.8wt%.

[0114] Exemplarily, in one embodiment, when the auxiliary agent includes a combination of a compatibilizer, a nucleating agent, a coupling agent and an antioxidant:

[0115] The weight of the compatibilizer is 2% of the weight of the resin matrix;

[0116] The weight of the nucleating agent is 0.08% of the weight of the polypropylene resin;

[0117] The weight of the antioxidant is 0.25% of the weight of the resin matrix;

[0118] The solute mass fraction of the coupling agent aqueous solution is 0.35 wt %.

[0119] In another embodiment, when the auxiliary agent includes a combination of a compatibilizer, a nucleating agent, a coupling agent and an antioxidant:

[0120] The weight of the compatibilizer is 4% of the weight of the resin matrix;

[0121] The weight of the nucleating agent is 0.1% of the weight of the polypropylene resin;

[0122] The weight of the antioxidant is 0.6% of the weight of the resin matrix;

[0123] The solute mass fraction of the coupling agent aqueous solution is 0.6 wt %.

[0124] In another embodiment, when the auxiliary agent includes a combination of a compatibilizer, a nucleating agent, a coupling agent and an antioxidant:

[0125] The weight of the compatibilizer is 6% of the weight of the resin matrix;

[0126] The weight of the nucleating agent is 0.20% of the weight of the polypropylene resin;

[0127] The weight of the antioxidant is 1% of the weight of the resin matrix;

[0128] The solute mass fraction of the coupling agent aqueous solution is 0.8 wt %.

[0129] In an exemplary embodiment, the reinforcing fibers include chopped carbon fibers, and the chopped carbon fiber single filaments have a diameter of 2-10 μm and a length of 1-2 mm.

[0130] In this embodiment, the chopped carbon fiber can better improve the impact strength and fatigue resistance of the composite material to improve the mechanical properties of the composite material. For example, the diameter of the chopped carbon fiber monofilament can be 2 μm, 5 μm or 10 μm, and the length can be 1 mm, 1.5 mm or 2 mm.

[0131] like Figure 1 As shown, an exemplary embodiment of the present application provides a method for preparing a composite material, the method for preparing a composite material is used to prepare the above fiber-reinforced polypropylene composite material, and the preparation method includes:

[0132] S110, mixing and granulating the resin matrix and the auxiliary agent under the first preset conditions to obtain composite resin particles.

[0133] When the auxiliary agent includes a combination of a compatibilizer, a nucleating agent, a coupling agent and an antioxidant, step S110 may be:

[0134] The resin matrix and the compatibilizer are mixed at a rotation speed of 400-500 r / min and a temperature of 110-130° C. for 10-20 minutes to obtain a premix; then an antioxidant and a nucleating agent are added to the premix, and mixed at a rotation speed of 500-800 r / min and a temperature of 75-85° C. for 5-15 minutes to obtain a mixture; the mixture is placed in a twin-screw extruder, and after melting, blending, extrusion, granulation, cooling and drying, composite resin particles are obtained; wherein the temperature of the twin-screw extruder is set at 175-230° C., the main engine speed is 20-40 r / min, and the feeding speed is 10-30 r / min.

[0135] Exemplarily, in one embodiment, S110 may be: mixing the resin matrix and the compatibilizer at a speed of 400 r / min and a temperature of 110°C for 20 minutes to obtain a premix; then adding an antioxidant and a nucleating agent to the premix, mixing at a speed of 500 r / min and a temperature of 75°C for 15 minutes to obtain a mixture; placing the mixture in a twin-screw extruder, and obtaining composite resin particles through melting, blending, extrusion, granulation, cooling, and drying; wherein the twin-screw extruder has a total of eleven temperature zones, and the temperatures in each zone are 175°C, 180°C, 185°C, 185°C, 190°C, 195°C, 205°C, 220°C, 230°C, 220°C, and 210°C, respectively; the main engine speed is 20 r / min, and the feeding speed is 10 r / min.

[0136] In another embodiment, S110 may be: mixing the resin matrix and the compatibilizer at a speed of 450 r / min and a temperature of 120°C for 15 minutes to obtain a premix; then adding an antioxidant and a nucleating agent to the premix, mixing at a speed of 600 r / min and a temperature of 80°C for 10 minutes to obtain a mixture; placing the mixture in a twin-screw extruder, and obtaining composite resin particles through melting, blending, extrusion, granulation, cooling, and drying; wherein the twin-screw extruder has eleven temperature zones, and the temperatures in each zone are 175°C, 180°C, 185°C, 185°C, 190°C, 195°C, 205°C, 220°C, 230°C, 220°C, and 210°C, respectively; the main engine speed is 30 r / min, and the feeding speed is 20 r / min.

[0137] In another embodiment, S110 may be: mixing the resin matrix and the compatibilizer at a speed of 500 r / min and a temperature of 130°C for 10 minutes to obtain a premix; then adding an antioxidant and a nucleating agent to the premix, mixing at a speed of 800 r / min and a temperature of 85°C for 5 minutes to obtain a mixture; placing the mixture in a twin-screw extruder, and obtaining composite resin particles through melting, blending, extrusion, granulation, cooling, and drying; wherein the twin-screw extruder has eleven temperature zones, and the temperatures in each zone are 175°C, 180°C, 185°C, 185°C, 190°C, 195°C, 205°C, 220°C, 230°C, 220°C, and 210°C, respectively; the main engine speed is 40r / min, and the feeding speed is 30r / min.

[0138] S120, mixing and granulating the composite resin particles and the reinforcing fibers under a second preset condition to obtain a fiber-reinforced polypropylene composite material.

[0139] Step S120 may be: mixing the composite resin particles and the reinforcing fibers uniformly at a rotation speed of 100-300 r / min and a temperature of 75-85° C. to obtain a blended material; placing the blended material in a twin-screw extruder, and performing melting, blending, extrusion, granulation, cooling, and drying to obtain a fiber-reinforced polypropylene composite material; wherein the temperature of the twin-screw extruder is set at 180-230° C., the main engine speed is 10-30 r / min, and the feeding speed is 10-20 r / min.

[0140] Exemplarily, in one embodiment, step S120 may be: mixing the composite resin particles and the reinforcing fibers uniformly at a rotation speed of 100 r / min and a temperature of 85°C to obtain a blended material; placing the blended material in a twin-screw extruder, and obtaining a fiber-reinforced polypropylene composite material through melting, blending, extrusion, granulation, cooling, and drying; wherein the twin-screw extruder temperature has eleven zones, and the temperatures in each zone are 180°C, 180°C, 185°C, 185°C, 190°C, 195°C, 205°C, 220°C, 230°C, 220°C, and 210°C, respectively; the main engine speed is 10 r / min, and the feeding speed is 10 r / min.

[0141] In another embodiment, step S120 may be: mixing the composite resin particles and the reinforcing fibers uniformly at a rotation speed of 200 r / min and a temperature of 80°C to obtain a blended material; placing the blended material in a twin-screw extruder, and performing melting, blending, extrusion, granulation, cooling, and drying to obtain a fiber-reinforced polypropylene composite material; wherein the twin-screw extruder temperature has eleven zones, and the temperatures in each zone are 180°C, 180°C, 185°C, 185°C, 190°C, 195°C, 205°C, 220°C, 230°C, 220°C, and 210°C, respectively; the main engine speed is 20 r / min, and the feeding speed is 15 r / min.

[0142] In another embodiment, step S120 may be: mixing the composite resin particles and the reinforcing fibers uniformly at a rotation speed of 300 r / min and a temperature of 75°C to obtain a blended material; placing the blended material in a twin-screw extruder, and performing melting, blending, extrusion, granulation, cooling, and drying to obtain a fiber-reinforced polypropylene composite material; wherein the twin-screw extruder temperature has eleven zones, and the temperatures in each zone are 180°C, 180°C, 185°C, 185°C, 190°C, 195°C, 205°C, 220°C, 230°C, 220°C, and 210°C, respectively; the main engine speed is 30 r / min, and the feeding speed is 20 r / min.

[0143] In an exemplary embodiment, before granulating the composite resin particles and the reinforcing fibers in step S110, the preparation method further includes:

[0144] The aqueous solution of the coupling agent is mixed with the initial fiber under the third preset condition and dried to obtain the reinforced fiber.

[0145] In this embodiment, the initial fibers are surface treated with an aqueous solution of a coupling agent to improve the interfacial compatibility between the initial fibers and the resin matrix, so that each raw material can be evenly dispersed and cracks in the product can be effectively prevented from expanding.

[0146] The third condition may be: soaking the initial fiber in the aqueous solution of the coupling agent for 1-3 hours; then drying the treated initial fiber in a vacuum drying oven at 110-130°C for 5-8 hours. The preparation method of the aqueous solution of the coupling agent is: diluting the coupling agent with deionized water and stirring at a temperature of 70-90°C for 5-15 minutes to obtain an aqueous solution of the coupling agent; the mass fraction of the solute in the aqueous solution of the coupling agent may be 0.35-0.8wt%.

[0147] Exemplarily, in one embodiment, the modification method of the reinforcing fiber includes:

[0148] The coupling agent was diluted with deionized water and stirred at 70° C. for 15 minutes to obtain an aqueous solution of the coupling agent; wherein the mass fraction of the solute in the aqueous solution of the coupling agent was 0.35 wt %.

[0149] The initial fibers were immersed in an aqueous solution of a coupling agent for 3 hours; the treated initial fibers were then dried in a vacuum drying oven at 110° C. for 8 hours to obtain reinforced fibers.

[0150] In another embodiment, the method for modifying the reinforcing fiber comprises:

[0151] The coupling agent was diluted with deionized water and stirred at 80° C. for 10 minutes to obtain an aqueous solution of the coupling agent; wherein the mass fraction of the solute in the aqueous solution of the coupling agent was 0.6 wt %.

[0152] The initial fibers were immersed in an aqueous solution of a coupling agent for 2 hours; the treated initial fibers were then dried in a vacuum drying oven at 120° C. for 6 hours to obtain reinforced fibers.

[0153] In another embodiment, the method for modifying the reinforcing fiber comprises:

[0154] The coupling agent was diluted with deionized water and stirred at 90° C. for 5 minutes to obtain an aqueous solution of the coupling agent; wherein the mass fraction of the solute in the aqueous solution of the coupling agent was 0.8 wt %.

[0155] The initial fibers were immersed in an aqueous solution of a coupling agent for 3 hours; the treated initial fibers were then dried in a vacuum drying oven at 130° C. for 5 hours to obtain reinforced fibers.

[0156] The specific implementation methods of the present application are further described below in conjunction with preferred embodiments, and examples of preferred value ranges of each component in the fiber-reinforced polypropylene composite material provided by the present application are explained in detail.

[0157] Preferred Example 1

[0158] A fiber-reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0159] 80-120 parts by weight of resin matrix;

[0160] 15-45 parts by weight of reinforcing fiber;

[0161] 2-15 parts by weight of auxiliary agent;

[0162] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

[0163] Preferred Example 2

[0164] A fiber-reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0165] 80-120 parts by weight of resin matrix;

[0166] 15-45 parts by weight of reinforcing fiber;

[0167] 2-15 parts by weight of auxiliary agent;

[0168] Wherein, the resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin;

[0169] The weight ratio of polypropylene resin to polyamide resin is 1.20-9.00:1;

[0170] The weight ratio of the homopolymer polypropylene resin to the block copolymer polypropylene resin is 1.05-1.55:1.

[0171] Preferred Example 3

[0172] A fiber-reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0173] 80-120 parts by weight of resin matrix;

[0174] 15-45 parts by weight of reinforcing fiber;

[0175] 2-15 parts by weight of auxiliary agent;

[0176] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin; the crystallinity of the homopolymer polypropylene resin is 43-48%; the crystallinity of the block copolymer polypropylene resin is 38-42%;

[0177] The weight ratio of polypropylene resin to polyamide resin is 1.20-9.00:1;

[0178] The weight ratio of the homopolymer polypropylene resin to the block copolymer polypropylene resin is 1.05-1.55:1;

[0179] The compatibilizer includes polypropylene grafted with maleic anhydride;

[0180] Nucleating agents include calcium phthaloyl beta-alaninate;

[0181] The coupling agent includes an aluminate coupling agent and a titanate coupling agent, and the weight ratio of the aluminate coupling agent to the titanate coupling agent is 1-3:1;

[0182] Antioxidants include pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].

[0183] Preferred Example 4

[0184] A fiber-reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0185] 80-120 parts by weight of resin matrix;

[0186] 15-45 parts by weight of reinforcing fiber;

[0187] 2-15 parts by weight of auxiliary agent;

[0188] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin; the crystallinity of the homopolymer polypropylene resin is 43-48%; the crystallinity of the block copolymer polypropylene resin is 38-42%;

[0189] The weight ratio of polypropylene resin to polyamide resin is 1.20-9.00:1;

[0190] The weight ratio of the homopolymer polypropylene resin to the block copolymer polypropylene resin is 1.05-1.55:1;

[0191] The reinforcing fibers include chopped carbon fibers, wherein the diameter of the chopped carbon fiber monofilament is 2-10 μm and the length is 1-2 mm;

[0192] The auxiliary agent includes a compatibilizer, a nucleating agent, a coupling agent and an antioxidant, wherein:

[0193] The compatibilizer includes polypropylene grafted maleic anhydride, and the weight of the compatibilizer is 2-6% of the weight of the resin matrix;

[0194] The nucleating agent includes calcium phthaloyl beta-alanine, and the weight of the nucleating agent is 0.08-0.20% of the weight of the polypropylene resin;

[0195] The coupling agent includes an aluminate coupling agent and a titanate coupling agent, the weight ratio of the aluminate coupling agent to the titanate coupling agent is 1-3:1, and the solute mass fraction of the coupling agent aqueous solution is 0.35-0.8wt%;

[0196] The antioxidant comprises pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and the weight of the antioxidant is 0.25-1% of the weight of the resin matrix.

[0197] Preferred Example 5

[0198] A fiber-reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0199] 80-90 parts by weight of resin matrix;

[0200] 20-40 parts by weight of reinforcing fiber;

[0201] 4-8 parts by weight of auxiliary agent;

[0202] The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin; the crystallinity of the homopolymer polypropylene resin is 43-48%; the crystallinity of the block copolymer polypropylene resin is 38-42%;

[0203] The weight ratio of polypropylene resin to polyamide resin is 1.86-3.20:1;

[0204] The weight ratio of the homopolymer polypropylene resin to the block copolymer polypropylene resin is 1.25-1.40:1;

[0205] The reinforcing fibers include chopped carbon fibers, wherein the diameter of the chopped carbon fiber monofilament is 2-10 μm and the length is 1-2 mm;

[0206] The auxiliary agent includes a compatibilizer, a nucleating agent, a coupling agent and an antioxidant, wherein:

[0207] The compatibilizer includes polypropylene grafted maleic anhydride, and the weight of the compatibilizer is 4.5-6% of the weight of the resin matrix;

[0208] The nucleating agent includes calcium phthaloyl beta-alanine, and the weight of the nucleating agent is 0.12-0.18% of the weight of the polypropylene resin;

[0209] The coupling agent includes an aluminate coupling agent and a titanate coupling agent, the weight ratio of the aluminate coupling agent to the titanate coupling agent is 1-3:1, and the solute mass fraction of the coupling agent aqueous solution is 0.35-0.8wt%;

[0210] The antioxidant comprises pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and the weight of the antioxidant is 0.5-1% of the weight of the resin matrix.

[0211] The method for preparing the composite material of preferred examples 1 to 5 comprises:

[0212] Mixing the resin matrix and the auxiliary agent under the first preset conditions to granulate to obtain composite resin particles;

[0213] The composite resin particles and the reinforcing fibers are mixed and granulated under a second preset condition to obtain a fiber-reinforced polypropylene composite material.

[0214] In order to more clearly explain the technical solution of the present application, the present application lists specific examples of fiber-reinforced polypropylene composite materials, and the beneficial effects of selecting the above-mentioned ranges of the contents of each component will be explained by providing specific experimental data through specific examples.

[0215] Example

[0216] It should be noted that, unless otherwise specified, the raw materials in the following examples can be obtained from commercial sources.

[0217] The crystallinity of the homopolymer polypropylene resin is 45%; the crystallinity of the block copolymer polypropylene resin is 40%; the polyamide resin is polyamide 6; the initial fiber used for the reinforcing fiber is short-cut carbon fiber with a single fiber diameter of 5 μm and an average length of 1.5 mm.

[0218] Embodiment 1: A method for preparing a fiber-reinforced polypropylene composite material, comprising the following steps:

[0219] (1) 38.9 kg of homopolymer polypropylene resin, 31.1 kg of block copolymer polypropylene resin, 30 kg of polyamide resin, and 4.5 kg of compatibilizer polypropylene grafted maleic anhydride were mixed in a high-speed mixer at a speed of 450 r / min and a temperature of 120° C. for 15 minutes to obtain a premix.

[0220] (2) 0.6 kg of antioxidant and 0.084 kg of nucleating agent were added to the premix, and the mixture was mixed at a speed of 500 r / min and a temperature of 75° C. for 15 min to obtain a mixture.

[0221] (3) placing the mixture in a twin-screw extruder, and performing melting, blending, extrusion, granulation, cooling, and drying to obtain composite resin particles; wherein the twin-screw extruder has eleven temperature zones, each zone temperature is 175 to 230° C., the main engine speed is 20 r / min, and the feed speed is 10 r / min.

[0222] (4) The coupling agent was diluted with deionized water and stirred at 80° C. for 10 min to obtain an aqueous solution of the coupling agent with a solute mass fraction of 0.35 wt %.

[0223] (5) The chopped carbon fibers are immersed in an aqueous solution of a coupling agent for 2 hours; the treated initial fibers are then dried in a vacuum drying oven at 120° C. for 6 hours to obtain reinforced fibers.

[0224] (6) The composite resin particles and 25 kg of reinforcing fibers were mixed uniformly at a rotation speed of 200 r / min and a temperature of 80° C. to obtain a blended material.

[0225] (7) placing the blended material in a twin-screw extruder, and performing melting, blending, extrusion, granulation, cooling, and drying to obtain a fiber-reinforced polypropylene composite material; wherein the temperature of the twin-screw extruder is set at 180-230° C., the main engine speed is 20 r / min, and the feed speed is 15 r / min.

[0226] In order to more clearly explain the technical solution of the present application, the present application also lists Examples 2-20 of the fiber-reinforced polypropylene composite material, wherein the formulas of Examples 2-20 are shown in Table 1.

[0227] Table 1 shows a specific embodiment of the fiber reinforced polypropylene composite material in the present application. It should be noted that, except for the parameters listed in Table 1, other parameters of Examples 2-20 are substantially the same as those of Example 1.

[0228] Wherein, the ratio C1 in Table 1 is the weight ratio of the homopolypropylene resin to the block copolymer polypropylene resin;

[0229] Ratio C2 is the weight ratio of polypropylene resin to polyamide resin;

[0230] The ratio C3 is the weight ratio of the resin matrix to the reinforcing fibers;

[0231] The ratio C4 is the weight ratio of the aluminate coupling agent to the titanate coupling agent.

[0232] Table 1 Raw material usage table of the embodiment

[0233]

[0234] Table 1 (Continued) Raw material usage table of the embodiment

[0235]

[0236] Table 1 (Continued) Raw material usage table of the embodiment

[0237]

[0238] Performance Testing

[0239] The properties of the composite material prepared in the example were tested according to the following method, and the test results are recorded in Table 2.

[0240] 1. Tensile properties: Tested in accordance with the method in GB / T 1040.2-2006 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics".

[0241] 2. Impact strength: Tested according to the method in GB / T 1843-2008 "Determination of cantilever beam impact strength of plastics".

[0242] 3. Heat resistance temperature: Tested according to the method in GB / T 19466.3-2004 "Plastics Differential Scanning Calorimetry (DSC) Part 3: Determination of Melting and Crystallization Temperature and Thermal Enthalpy".

[0243] Table 2 Performance test table of the composite material of the embodiment

[0244]

[0245] Combining the data of Examples 1-20 in Table 1 and Table 2, it can be seen that when the amount and ratio of each raw material change, the mechanical properties and heat resistance of the composite material are greatly affected. The composite material prepared by the method of the embodiment of the present application has a tensile strength of ≥160MPa, a tensile modulus of ≥900MPa, and an impact strength of ≥7.0kJ / m 2 , the heat-resistant temperature is ≥210°C, indicating that the composite material of the present application has excellent tensile properties, impact resistance and thermal stability.

[0246] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0247] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application is described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A fiber-reinforced polypropylene composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 80-120 parts by weight of resin matrix; 15-45 parts by weight of reinforcing fiber; 2-15 parts by weight of auxiliary agent; The resin matrix includes polypropylene resin and polyamide resin, and the polypropylene resin includes homopolymer polypropylene resin and block copolymer polypropylene resin.

2. The fiber-reinforced polypropylene composite material according to claim 1, characterized in that: The weight ratio of the polypropylene resin to the polyamide resin is 1.20-9.00:

1.

3. The fiber-reinforced polypropylene composite material according to claim 1 or 2, characterized in that: The weight ratio of the homopolymer polypropylene resin to the block copolymer polypropylene resin is 1.05-1.55:

1.

4. The fiber-reinforced polypropylene composite material according to claim 1, characterized in that: The crystallinity of the homopolymer polypropylene resin is 43-48%; the crystallinity of the block copolymer polypropylene resin is 38-42%.

5. The fiber-reinforced polypropylene composite material according to claim 1, characterized in that: The auxiliary agent includes a combination of one or more of a compatibilizer, a nucleating agent, a coupling agent, and an antioxidant.

6. The fiber-reinforced polypropylene composite material according to claim 5, characterized in that: When the auxiliary agent comprises a combination of the compatibilizer, the nucleating agent, the coupling agent and the antioxidant: The compatibilizer includes polypropylene grafted with maleic anhydride; The nucleating agent includes calcium phthaloyl beta-alaninate; The coupling agent includes an aluminate coupling agent and a titanate coupling agent, and the weight ratio of the aluminate coupling agent to the titanate coupling agent is 1-3:1; The antioxidant includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].

7. The fiber-reinforced polypropylene composite material according to claim 5, characterized in that: When the auxiliary agent is a composition comprising the compatibilizer, the nucleating agent, the coupling agent and the antioxidant: The weight of the compatibilizer is 2-6% of the weight of the resin matrix; The weight of the nucleating agent is 0.08-0.20% of the weight of the polypropylene resin; The weight of the antioxidant is 0.25-1% of the weight of the resin matrix; The solute mass fraction of the aqueous solution of the coupling agent is 0.35-0.8 wt %.

8. The fiber-reinforced polypropylene composite material according to claim 1, characterized in that: The reinforcing fibers include chopped carbon fibers, wherein the chopped carbon fiber monofilament has a diameter of 2-10 μm and a length of 1-2 mm.

9. A method for preparing a composite material, characterized in that: The preparation method of the composite material is used to prepare the fiber-reinforced polypropylene composite material according to any one of claims 1 to 8, and the preparation method comprises: Mixing and granulating the resin matrix and the auxiliary agent under a first preset condition to obtain composite resin particles; The composite resin particles and the reinforcing fibers are mixed and granulated under a second preset condition to obtain the fiber-reinforced polypropylene composite material.

10. The method for preparing a composite material according to claim 9, characterized in that: Before granulating the composite resin particles and the reinforcing fibers after mixing, the preparation method further comprises: The reinforcing fibers are obtained by mixing the aqueous solution of the coupling agent with the initial fibers under the third preset condition and drying them.