Transparent fluoride-free lyophobic antifouling coating and preparation method thereof
By forming a gradient gradient structure of transition layer, SiO2-like structure and PDMS-like structure on the plating substrate, the existing oleophobic coating has been solved in terms of durability and chemical uniformity, and high transparency and mechanical durability have been achieved. Transparent fluorine-free liquid-repellent anti-fouling coating, with excellent dynamic liquid-repellent properties and hardness.
Patent Information
- Application Number
- CN202411044248.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing oleophobic coatings have shortcomings in terms of durability and chemical uniformity, especially in the preparation process of liquid-like surface coatings, due to the steric hindrance effect, the surface is uneven, and the durability and mechanical properties are poor, making it difficult to actually be It exhibits good liquid repellency during application.
Using a transparent fluorophobic anti-fouling coating, a gradient gradient structure with transition layer, SiO2-like structure and PDMS-like structure are formed on the plating substrate, and continuously prepared by gas phase method to adjust the silicon/oxygen ratio and organic/inorganic structure. The proportion is to form a coating with high transparency and mechanical durability.
It achieves high transparency, excellent dynamic liquid repellency and mechanical durability, low surface roughness reduces droplet sliding resistance, and gradient gradient structure improves the hardness and wear resistance of the coating, ensuring the long-term use of the coating stability.
Smart Images

Figure CN118909466A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer coatings, and in particular to a transparent fluorine-free liquid-repellent antifouling coating and a preparation method thereof. Background Art
[0002] The role of hydrophobic and oleophobic coatings in daily life and industry is very important, and they have potential applications in anti-fouling, anti-corrosion, anti-icing, separation and other fields. It mainly achieves the hydrophobic and oleophobic effect by reducing the surface energy of the material surface. The surface tension of oil is lower, generally between 20 and 30 mN / m, so the preparation of oleophobic coatings is more difficult than that of hydrophobic coatings. Currently, oleophobic coatings are often prepared using fluorinated polymers, but fluorinated polymers are often bioaccumulative and have a greater impact on the human body and the environment, so their use is gradually being restricted by regulations.
[0003] There are three main methods for preparing oleophobic surfaces: double superphobic coatings, liquid surfaces, and liquid-like surfaces. 1) The preparation of super double oleophobic coatings (SHPS / SOPS) mainly adopts a combination of low surface energy coatings and micro-nano structures, using the air layer to achieve a lyophobic effect. However, the instability of the air layer will lose its original function under higher pressures; and the micro-nano structure is easily destroyed and difficult to restore, making this type of coating less durable. 2) Liquid surfaces represented by liquid-injected surfaces (SL IPS) use low surface energy lubricants to inject into porous surfaces to form a smooth liquid layer on their surface, which enables this type of coating to resist any liquid that is incompatible with the lubricant. However, there are problems such as lubricant volatilization and contamination that can lead to performance failure, restricting long-term use. 3) In addition to the above two coatings, there is also a liquid-like surface (LLS) with tethered flexible polymer chains on the surface. The flexible polymer chains on its surface undergo conformational rearrangement when in contact with liquids with low surface tension, thereby producing dynamic oleophobic properties. Moreover, the liquid-like surface does not need to consider the loss of surface micro-nanostructure and surface lubricant, so it has significant advantages over the previous two in practical applications.
[0004] However, liquid-like surfaces are often prepared by grafting and other methods, resulting in a small coating thickness and a size of only a few to tens of nanometers, which limits the mechanical durability to a certain extent. In addition, due to the steric hindrance effect during the grafting process, the flexible polymer segments on the surface will have uneven coverage, resulting in surface chemical heterogeneity, and affected by the surface roughness of the substrate, structural heterogeneity will occur, which makes it very easy for pinning to occur during the liquid-repellent process, hindering the sliding of droplets.
[0005] Therefore, it is of great significance to develop a durable fluorine-free liquid surface having good liquid-repelling (hydrophobic and oleophobic) effect, surface self-smoothing function and chemical uniformity. Summary of the invention
[0006] The present invention aims to provide a transparent fluorine-free liquid-repellent antifouling coating and a preparation method thereof to solve the deficiencies in the prior art. The technical problem to be solved by the present invention is achieved through the following technical solutions.
[0007] On the one hand, the present invention proposes a transparent fluorine-free liquid-phobic antifouling coating, wherein the transition layer adopts an organic coating with different structural main chains according to different coating substrates; the antifouling coating includes a gradient structure of a transition layer, a SiO2-like structure and a PDMS-like structure, the SiO2-like structure is the main part of the coating, wherein the organic / inorganic structure accounts for 0.05 to 0.3, and the silicon / oxygen element ratio is in the range of 0.28 to 0.38; the PDMS-like structure includes periodic Si(CH3)2 repeating units, wherein the organic / inorganic structure accounts for 0.4 to 3.0, and the silicon / oxygen element ratio is between 0.4 and 0.7.
[0008] Further, the coating substrate is an inorganic material or an organic material, the inorganic material is selected from glass, ceramic, stainless steel, copper, aluminum, and iron, and the organic material is selected from polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC), acrylonitrile-butadiene-styrene (ABS), polystyrene (PS), polycarbonate (PC), polyurethane (PU), rubber, natural polymer or PMMA;
[0009] When the plating substrate is made of inorganic material, the transition layer is an organic silicon coating with Si and O as the main chain; when the plating substrate is made of organic material, the transition layer is an organic coating with CC chain as the main chain.
[0010] Furthermore, the inner structure of the antifouling coating gradually changes from the PDMS-like structure of the transition layer to the SiO2-like structure and then to the PDMS-like structure.
[0011] Furthermore, the proportion of Si-(O)3 and Si-(O)4 in the SiO2-like structure is in the range of 70-95%.
[0012] Furthermore, the organic / inorganic structure ratio is used to characterize the Silicon bonding.
[0013] Furthermore, the transition layer, the SiO2-like structure and the PDMS-like structure are all continuously prepared by a gas phase method.
[0014] Another aspect of the present invention provides a method for preparing a transparent fluorine-free liquid-repellent antifouling coating, comprising the following steps:
[0015] S1: After cleaning and drying, the substrate is placed in a plasma chamber, and then the chamber is closed and vacuumed;
[0016] S2: introducing activation gas, inputting plasma, cleaning and activating the substrate surface again, increasing the substrate surface temperature, and then closing the plasma and exhausting the additional gas;
[0017] S3: introducing precursor A and auxiliary reaction gas D, inputting plasma, and completing the deposition of plasma polymer transition layer;
[0018] S4: adjusting the plasma power and deposition pressure, inputting the precursor B and the auxiliary reaction gas E for deposition at the same time, and then closing the auxiliary reaction gas D and the precursor A in turn to complete the deposition of the SiO2-like layer with a cross-linked structure;
[0019] S5: adjusting the deposition pressure, introducing the precursor C, depositing for several minutes, turning off the precursor B, adjusting the plasma power, depositing for several minutes, turning off the plasma input and all monomer inputs, exhausting the exhaust gas, breaking the vacuum, and then completing the preparation of the linear PDMS-like layer with a structural gradient;
[0020] The deposition process from step S3 to step S5 is continuous and uninterrupted.
[0021] The precursor A has one or a mixture of two or more of a linear hydrocarbon and a linear organosilane system, and has a saturated vapor pressure of not less than 2.5 kPa at 20° C., including but not limited to the following monomers: tetraethyl orthosilicate, pentamethyldisiloxane, hexamethyldisiloxane, hexamethyldisilazane, bistrimethylsiloxymethylsilane, octamethyltrisiloxane, 1,1,3,3-tetramethyldisiloxane, tetramethyldivinyldisiloxane, vinylpentamethyldisiloxane, 1,3-diethyl-1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-divinyl-hexamethyltrisiloxane, 1-vinyl-1,1,3,3-tetramethyldisiloxane, silane, methane, ethane, hexafluoropropylene, hexafluorobutyl acrylate, acrylic acid, butyl methacrylate;
[0022] The precursor B is one or a mixture of two or more organic silane monomers having one or two or more rings. The relative silicon content in the precursor B is greater than 40%, and the saturated vapor pressure is not less than 0.1 kPa at 20°C, including but not limited to the following monomers: 2,4,6-trivinyl-2,4,6-trimethylcyclotrisiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, octamethylcyclotetrasiloxane, 2,4,6,8-tetramethyltetravinylcyclotetrasiloxane, heptamethylcyclotetrasiloxane, 2,4,6,8,10-cyclopentasiloxane, acetoxyheptamethylcyclotetrasiloxane;
[0023] The precursor C is a linear organic silicon monomer with a main chain of -Si-O-, including but not limited to the following monomers: pentamethyldisiloxane, hexamethyldisiloxane, bistrimethylsiloxymethylsilane, octamethyltrisiloxane, 1,1,3,3-tetramethyldisiloxane, tetramethyldivinyldisiloxane, vinylpentamethyldisiloxane, 1,3-diethyl-1,1,3,3-tetramethyldisiloxane, 1-allyl-1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-divinyl-hexamethyltrisiloxane, 1-vinyl-1,1,3,3-tetramethyldisiloxane, 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane.
[0024] The auxiliary reaction gases D and E are one or a mixture of two or more of Ar, O2, N2, H2O, H2O2, and H2.
[0025] Furthermore, the time interval from closing the auxiliary reaction gas D and opening the precursor C to closing the precursor B is 10 to 300 seconds, and the deposition time from closing the precursor B to the end of deposition is 60 to 900 seconds.
[0026] The "liquid-like" coating of the present invention has high transparency, excellent dynamic liquid-repellent properties and mechanical durability. The dynamic liquid-repellent ("liquid-like") property is mainly attributed to: 1) the PDMS-like structure (i.e., Si(O)2 structure) on its surface has good fluidity at room temperature, and the polymer chains on the surface will undergo conformational rearrangement when in contact with droplets, resulting in regional surface energy unevenness at the triple line, which helps the droplets to slide quickly at extremely low tilt angles; 2) The surface has extremely low roughness (sub-nanometer level), which significantly reduces the resistance of the droplets during sliding. The low surface roughness also ensures extremely low light scattering and high light transmittance. The SiO2-like structure in the gradient structure of the coating gives the coating excellent mechanical properties, making it have extremely high hardness and wear resistance compared to ordinary polymer coatings.
[0027] The present invention has a gradient structure, that is, there is a component at the top of the coating that gradually changes from a high cross-linked structure to a low cross-linked structure. The high cross-linked area (SiO2-like structure layer) has high hardness and rigidity, which can resist external forces, and the low cross-linked area (PDMS-like structure layer) provides the coating with good liquid-repellent properties. However, the gradient structure effectively alleviates problems such as modulus mismatch between coatings of different structures. The coating reduces internal stress mismatch when resisting external forces, effectively improving problems such as internal delamination and cracking of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The SEM images of (a) Example 1, (b) Example 2 and (c) Comparative Example 1;
[0029] Figure 2 AFM images of (a) Example 1 and (b) Comparative Example 1;
[0030] Figure 3 It is the UV-vis diagram of Example 1 and Comparative Example 1;
[0031] Figure 4 are cross-sectional views of (a) Example 1 and (b) Comparative Example 1;
[0032] Figure 5 Si 2p diagrams of (a) SiO2-like structure and (b) PDMS-like structure of Example 1;
[0033] Figure 6 is the sliding angle after the friction test of Example 1, Comparative Example 5, Comparative Example 7 and Comparative Example 8;
[0034] Figure 7 XPS in-depth element analysis of Example 1;
[0035] Figure 8 The antifouling test of Example 2;
[0036] Fig. 9 The repelling effect of chili oil on the glass after coating with the coating of Example 2;
[0037] Fig.10 Example 2 shows the repelling effect of quick-drying ink. DETAILED DESCRIPTION
[0038] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0039] A specific embodiment of the present invention provides a transparent fluorine-free liquid-repellent antifouling coating, including a transition layer, a SiO2-like structure and a PDMS-like structure. The structure in the coating gradually changes from the transition layer to the SiO2-like structure and then to the PDMS-like structure. The SiO2-like structure is the main part of the coating, in which the organic / inorganic structure accounts for a certain proportion (characterizing the silicon bonding in the test). The ratio of silicon to oxygen is between 0.05 and 0.3, and the ratio of silicon to oxygen is between 0.28 and 0.38. This part of the structure has a higher SiO bond and cross-linking unit, so it has greater rigidity and better mechanical properties. The PDMS-like structure includes periodic Si(CH3)2 repeating units, in which the organic / inorganic structure accounts for The ratio of silicon to oxygen is between 0.4 and 3.0, and the ratio of silicon to oxygen is between 0.4 and 0.7. There are more Si(CH3)2 repeating units in the structure. The coating composed of this partial structure has a lower glass transition temperature. The polymer chain has high fluidity at room temperature. When it comes into contact with droplets, it will undergo conformational rearrangement, resulting in uneven surface energy in the region at the solid-liquid-gas triple line, reducing the resistance of the droplets when they slide, so that the droplets can quickly slide off the surface at extremely low tilt angles.
[0040] The three-layer structure required by the present invention includes a transition layer, a SiO2-like structure layer and a PDMS-like structure layer. The three layers are prepared continuously by a gas phase method, and a large number of residual active sites are required on the surface of the transition layer after preparation, and the surface structure of the SiO2-like structure layer is regulated by the residual active sites. If there is no transition layer, the SiO2-like structure layer will produce a large number of disordered structures, affecting the final coating performance. The transition layer should use organic coatings with different structural main chains for the plating substrate. For example, when plating on the surface of glass and other objects, the transition layer should be an organic silicon coating with Si, O as the main chain; when plating on a substrate of a material such as PMMA (organic glass), the transition layer should be an organic coating with CC chain as the main chain; the structure and composition of the transition layer similar to the substrate can ensure that the prepared coating and the substrate have a good match, avoiding cracking and blistering of the coating under harsh conditions of use.
[0041] The coating of this embodiment has good liquid-repellent properties, with a sliding angle of water (20 μL) <10°, a sliding angle of other liquids (10 μL) <6°, a light transmittance >90%, and a light transmittance >99.5% after deducting the substrate.
[0042] The specific preparation method of the above coating is described in detail below, including the following steps:
[0043] S1: Different substrates are cleaned and dried using different methods according to their respective properties, and then placed in a plasma chamber. The chamber is closed and a mechanical pump is turned on for vacuuming.
[0044] The substrate materials include, but are not limited to, polymer materials such as polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC), acrylonitrile-butadiene-styrene (ABS), polystyrene (PS), polycarbonate (PC), polyurethane (PU), rubber, natural polymers, inorganic non-metallic materials such as glass and ceramics, metal materials such as stainless steel, copper, aluminum, iron, circuit boards, micro / small sensors, and other devices. Its shapes include, but are not limited to, spherical, regular, irregular, etc.
[0045] S2: Introduce activation gas, input plasma, clean and activate the surface of the substrate again, increase the substrate surface temperature appropriately, and then turn off the plasma and exhaust the additional gas.
[0046] The activation gas is one or a mixture of two or more of O2, N2, He, Ar, and Ne. In this embodiment, the activation gas is O2 and Ar.
[0047] S3: introducing precursor A and auxiliary reaction gas D, inputting plasma, and depositing for several minutes to complete the deposition of the plasma polymer transition layer.
[0048] Precursor A is a mixture of one or more of a linear hydrocarbon and a linear organosilane system, and the saturated vapor pressure is not less than 2.5 kPa at 20° C. Precursor A includes but is not limited to the following monomers: tetraethyl orthosilicate, pentamethyldisiloxane, hexamethyldisiloxane, hexamethyldisilazane, bistrimethylsiloxymethylsilane, octamethyltrisiloxane, 1,1,3,3-tetramethyldisiloxane, tetramethyldivinyldisiloxane, vinylpentamethyldisiloxane, dimethoxymethylvinylsilane, 1,3-diethyl-1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-divinyl-hexamethyltrisiloxane, 1-vinyl-1,1,3,3-tetramethyldisiloxane, silane, methane, ethane, hexafluoropropylene, hexafluorobutyl acrylate, acrylic acid, and butyl methacrylate. Precursor A is preferably a silicon / carbon-containing monomer with a linear structure and a low silicon content, which is beneficial to improving the surface uniformity of the prepared coating and reducing the roughness.
[0049] The auxiliary reaction gas D is one of Ar, O2, N2, H2O, H2O2, H2, or a mixture of two or more thereof. In this embodiment, the auxiliary reaction gas D is Ar, O2, or N2.
[0050] S4: Adjust the plasma power and deposition pressure, input the precursor B and the auxiliary reaction gas E at the same time, turn off the auxiliary reaction gas D and the precursor A in turn, deposit for several minutes, and complete the deposition of the cross-linked structured SiO2-like layer.
[0051] The auxiliary reaction gas E is one of Ar, O2, N2, H2O, H2O2, H2, or a mixture of two or more thereof. In this embodiment, the auxiliary reaction gas E is Ar or O2.
[0052] Precursor B is one or a mixture of two or more organic silane monomers having one or two or more rings. The relative silicon content in precursor B is greater than 40%, and the saturated vapor pressure is not less than 0.1 kPa at 20°C. Precursor B includes but is not limited to the following monomers: 2,4,6-trivinyl-2,4,6-trimethylcyclotrisiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, octamethylcyclotetrasiloxane, 2,4,6,8-tetramethyltetravinylcyclotetrasiloxane, heptamethylcyclotetrasiloxane, 2,4,6,8,10-cyclopentasiloxane, acetoxyheptamethylcyclotetrasiloxane.
[0053] In this embodiment, the auxiliary reaction gases D and E are O2. In other embodiments, the auxiliary reaction gases D and E are one or a mixture of two or more of Ar, O2, N2, H2O, H2O2, CH4, C2H2. Preferably, the auxiliary reaction gas D is Ar, O2, H2O, H2O2, and the auxiliary reaction gas E is Ar, O2.
[0054] The coating deposited in step S4 is a hard SiO2-like coating with a cross-linked structure, which improves the hardness of the overall coating. Properly increasing the pressure and power and reducing the flow rate can extend the residence time of the cracked particles on the substrate surface, and the formed -SiO- network is more inclined to Si(O)4, increasing the density of the coating, and the formed coating is used for higher hardness.
[0055] The silicon molar mass of the precursor B in step S4 accounts for more than 40%, and Si cannot be discharged from the cavity in the form of SiH4 gas, which makes the deposition rate of the precursor B greater than that of the precursor A. And the precursor B contains a -SiO- polycyclic structure. When the coating is deposited at a low plasma power density, the -SiO- ring structure is not easy to open due to the large bond energy of the -SiO- bond, and is easy to form an active polycyclic structure with a high adhesion rate, which is very easy to aggregate, and the coating grows on the substrate surface in a Volmer-Weber or Stranski-Krastanov manner, and the surface roughness is large.
[0056] However, since the smooth coating of linear precursor A in step S3 is first deposited as a transition layer, the density of free radicals on the substrate surface is increased, and when precursor A is deposited, precursor A is cracked to produce free hydrogen, which reacts with the deposited coating, increases the surface active sites, and can also increase the substrate surface temperature. Therefore, when the precursor B with a high silicon content is continuously deposited, the free radical sites on the surface inhibit the diffusion and aggregation of the active multi-ring structure on the substrate surface, so that the precursor B grows the coating in the Frank van der Merwe manner, reducing the generation of surface roughness structures.
[0057] S5: Adjust the deposition pressure, introduce precursor C, deposit for several minutes, turn off precursor B, adjust the plasma power, deposit for several minutes, turn off the plasma input and all monomer inputs, exhaust the exhaust gas, break the vacuum, and then complete the preparation of the linear PDMS layer with a structural gradient.
[0058] In the above step S5, the precursor C is a linear organic silicon monomer with a main chain of -SiO-, including but not limited to the following monomers: pentamethyldisiloxane, hexamethyldisiloxane, bistrimethylsiloxymethylsilane, octamethyltrisiloxane, 1,1,3,3-tetramethyldisiloxane, tetramethyldivinyldisiloxane, vinylpentamethyldisiloxane, 1,3-diethyl-1,1,3,3-tetramethyldisiloxane, 1-allyl-1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-divinyl-hexamethyltrisiloxane, 1-vinyl-1,1,3,3-tetramethyldisiloxane, and 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane.
[0059] In a preferred embodiment, the precursor C contains one or two or more weak bonds, including but not limited to silicon-hydrogen bonds, carbon-carbon double bonds, hydroxyl groups, amino groups, carboxyl groups, and halogen bonds.
[0060] In the above step S5, the time interval from closing the auxiliary reaction gas D, opening the precursor C to closing the precursor B is 10 to 300 seconds; in the present embodiment, the time interval is 60 to 180 seconds, and the flow rate of the precursor C is 10 to 20 sccm. After closing the auxiliary reaction gas D, the adjusted pressure is 30 to 200 Pa; in the present embodiment, the adjusted pressure is 50 to 100 Pa. The deposition time from closing the precursor B to the end of the deposition is 60 to 900 seconds; in the present embodiment, the deposition time is 300 to 600 seconds. After closing the precursor B, the plasma power density is adjusted to 1.0 to 5.0 kW / m 2 In this embodiment, the plasma power density is 1.0-2.0 kW / m 2 , the pressure remains at 50~100Pa.
[0061] When depositing a linear structured PDMS-like layer in the above step S5, the input plasma power and deposition pressure should not be too high, so that the prepared PDMS-like layer can have as many -O-Si-O-chains as possible, and a certain high number ratio of high-fluidity PDMS polymer chains (repeating units ≥ 15) is formed on the surface.
[0062] The deposition process from step S3 to step S5 is continuous and uninterrupted.
[0063] The present invention will be further described in detail below in conjunction with Examples 1-5 and Comparative Examples 1-8.
[0064] Example 1: Wash and dry the glass slide, silicon wafer, polycarbonate, and polished stainless steel plate (2.5×2.5 cm) and hang them on the sample rack as required. Close the chamber and turn on the mechanical pump to evacuate the pressure to 1 Pa. Open the chamber and rotate it. O2:Ar flow rate ratio of 1:4 is introduced into the chamber. 3.0 kW / m 2 The substrate was cleaned and activated for 300 seconds with plasma, the temperature was raised to 50°C, and then the chamber pressure was pumped back to 1 Pa. Precursor A and auxiliary gas D were turned on. In this embodiment, precursor A was dimethoxymethylvinylsilane, the flow ratio was 2:1, the total flow was 15 sccm, the pressure was maintained at 50 Pa, plasma was input, and the plasma power was adjusted to 4.0 kW / m 2 , deposit the transition layer for 600s. Then turn off the precursor A and auxiliary gas D, turn on the precursor B and auxiliary gas E. In this embodiment, the precursor B is octamethylcyclotetrasiloxane, the flow ratio is 1:1, the total flow is 10sccm, the reaction pressure is 70Pa, and the plasma power density is adjusted to 3.0kW / m 2 , the deposition time is 600s. Then the auxiliary gas E is turned off, and the precursor C is turned on. In this embodiment, the precursor C is 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane, the flow rate is 10sccm, the reaction pressure is 50Pa, and the plasma power is adjusted to 2.0kW / m 2 , the deposition time is 60s. Turn off precursor B and adjust the plasma power to 1.5kW / m 2 , maintain the pressure at 50Pa, deposit for 300s, then complete the preparation of the coating, close the air intake and plasma input, exhaust the exhaust gas in the chamber to below 10Pa, turn off the vacuum pump, break the vacuum, open the chamber, turn off the rotation, and take out the sample.
[0065] Example 2: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. The ratio of precursor B and auxiliary gas E in step S4 was adjusted to 1:2, the total flow rate was 10 sccm, the reaction pressure was adjusted to 100 Pa, and the plasma power density was adjusted to 6.5 kW / m 2 , the rest of the process is the same as in Example 1.
[0066] Example 3: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. The ratio of precursor B and auxiliary gas E in step S4 was adjusted to 3:1, the total flow rate was 10 sccm, the reaction pressure was 50 Pa, and the plasma power density was adjusted to 2.0 kW / m 2 , the rest of the process is the same as in Example 1.
[0067] Example 4: The same substrate as in Example 1 is hung in the chamber and evacuated to the same vacuum degree. The reaction pressure in step S5 is adjusted to 150 Pa, and the plasma power density after closing the precursor B is adjusted to 4.0 kW / m 2 , the deposition time was adjusted to 600 s, and the rest of the process was the same as in Example 1.
[0068] Example 5: The same substrate as in Example 1 is hung in the chamber and evacuated to the same vacuum degree. After turning off precursor B in step S5, the flow rate of precursor C is increased to 20 sccm, and the plasma power density after turning off precursor B is adjusted to 1.0 kW / m 2 , the deposition time was adjusted to 600 s, and the rest of the process was the same as in Example 1.
[0069] Table 1 shows the organic / inorganic structure ratio and silicon / oxygen element ratio of each sample in Example 1 to Example 5. The internal structure of the coating obtained in Example 1 gradually changes from the PDMS-like structure of the transition layer to the SiO2-like structure and then to the PDMS-like structure. The SiO2-like structure, the organic / inorganic structure ratio (characterizing the silicon bonding in the test) The ratio of silicon to oxygen is 0.12, and the ratio of silicon to oxygen is 0.286. The PDMS-like structure includes periodic Si(CH3)2 repeating units, in which the organic / inorganic structure accounts for The ratio of organic / inorganic structure to SiO2 structure in Example 2 is 0.05, and the ratio of organic / inorganic structure to PDMS structure is 0.75; the ratio of organic / inorganic structure to SiO2 structure in Example 3 is 0.3, and the ratio of organic / inorganic structure to PDMS structure is 0.73; the ratio of organic / inorganic structure to SiO2 structure in Example 4 is 0.124, and the ratio of organic / inorganic structure to PDMS structure is 0.4; the ratio of organic / inorganic structure to SiO2 structure in Example 5 is 0.131, and the ratio of organic / inorganic structure to PDMS structure is 3.
[0070] Table 1 Organic / inorganic structure ratio and silicon / oxygen element ratio of Example 1 to Example 5
[0071]
[0072]
[0073] Comparative Example 1: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. Step S3 was not performed, and the rest of the process was the same as in Example 1. The obtained coating structure included a SiO2-like structure and a PDMS-like structure, but did not contain a transition layer. The organic / inorganic structure ratio in the SiO2-like structure (characterizing the silicon bonding in the test) was ratio) is 0.128, and the silicon / oxygen element ratio is in the range of 0.284.
[0074] Comparative Example 2: The same substrate as in Example 1 is hung in the cavity and evacuated to the same vacuum degree. Step S4 is not performed, and the rest of the process is the same as in Example 1. The obtained coating structure includes a transition layer and a PDMS-like structure, but does not contain a SiO2-like structure. The PDMS-like structure includes periodic Si(CH3)2 repeating units, in which the organic / inorganic structure accounts for The element ratio of silicon to oxygen is 0.72 and 0.45.
[0075] Comparative Example 3: The same substrate as in Example 1 is hung in the cavity and evacuated to the same vacuum degree. Step S5 is not performed, and the rest of the process is the same as in Example 1. The obtained coating structure includes a SiO2-like structure and a transition layer, but does not contain a PDMS-like structure. The PDMS-like structure includes periodic Si(CH3)2 repeating units, in which the organic / inorganic structure accounts for The element ratio of silicon to oxygen is 0.131 and 0.287.
[0076] Comparative Example 4: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. The ratio of precursor B and auxiliary gas E in step S4 was adjusted to 3:7, the total flow rate was 10 sccm, the reaction pressure was adjusted to 100 Pa, and the plasma power density was adjusted to 6.0 kW / m 2 , the rest of the process is the same as in Example 1. The ratio of organic / inorganic structure of SiO2-like structure is 0.04, the ratio of organic / inorganic structure of PDMS-like structure It is 0.73.
[0077] Comparative Example 5: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. The ratio of precursor B and auxiliary gas E in step S4 was adjusted to 5:1, the total flow rate was 10 sccm, the reaction pressure was adjusted to 50 Pa, and the plasma power density was adjusted to 1.0 kW / m 2 , the rest of the process is the same as in Example 1. The ratio of organic / inorganic structure of SiO2-like structure is 0.6, the ratio of organic / inorganic structure of PDMS-like structure It is 0.72.
[0078] Comparative Example 6: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. The flow rate of precursor C in step S5 was adjusted to 5 sccm, the reaction pressure was adjusted to 100 Pa, and the plasma power density after closing precursor B was adjusted to 3.0 kW / m 2, the deposition time was adjusted to 600s, and the rest of the process was the same as in Example 1. The proportion of organic / inorganic structures of SiO2-like structures is 0.15, the ratio of organic / inorganic structure of PDMS-like structure is 0.35.
[0079] Comparative Example 7: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. After the precursor B was turned off in step S5, the flow rate of the precursor C was increased to 20 sccm, the reaction pressure was adjusted to 30 Pa, and the plasma power density after the precursor B was turned off was adjusted to 0.5 kW / m 2 , the deposition time was adjusted to 600s, and the rest of the process was the same as in Example 1. Ratio of organic / inorganic structure of SiO2-like structure is 0.14, the ratio of organic / inorganic structure of PDMS-like structure is 3.3.
[0080] Comparative Example 8: The same substrate as in Example 1 was hung in the chamber and evacuated to the same vacuum degree. Step S5 was changed to: turn off the plasma input, turn off the precursor B and the auxiliary reaction gas D, evacuate the chamber pressure to 1 Pa, and maintain it for 600 s, and then introduce the precursor C with a flow rate of 10 sccm, a reaction pressure of 50 Pa, and a plasma power of 1.5 kW / m 2 , the pressure was maintained at 50 Pa, the deposition was continued for 300 s, and the rest of the process was the same as in Example 1. is 0.14, the ratio of organic / inorganic structure of PDMS-like structure It is 0.71.
[0081] The UV-visible transmittance of the coatings deposited on glass in Example 1 and Comparative Example 1 was tested. When the precursor B was directly deposited without a transition layer, a large number of rough microstructures were generated on the surface, such as Figure 1 and Figure 2 As shown in the figure, it will seriously affect the light transmittance of the coating, which also shows the significance of the existence of the transition layer. Figure 3 As shown, after deducting the substrate, the transmittance of Example 1 in the visible light range (390-780nm) is greater than 99.5%; while in Comparative Example 1, due to the absence of a transition layer, the SiO2-like structural layer produces a micro-nano structure, which increases the reflection of light on its surface and reduces the overall transmittance.
[0082] like Figure 5 As shown in Table 2, after XPS analysis, the Si 2p spectra of the SiO2-like structure and the PDMS-like structure in Example 1 were obtained, and the proportions of different bonding of silicon elements were calculated, and the proportions of organic / inorganic structures in the coating structure were calculated based on this. The percentage of SiO bond energy is 101.1eV, Si-(O)2 bond energy is 102.1eV, Si-(O)3 bond energy is 102.8eV, and Si-(O)4 bond energy is 103.4eV. (The XPS test sample of the SiO2-like structure is the sample of Example 1 without step S5 deposition). Table 2 The area of different bonding states after Si 2p spectrum peak separation of the SiO2-like structure and the PDMS-like structure in Example 1 and the percentage of each organic / inorganic structure
[0083]
[0084] Referring to the national standard GB / T 24368-2229, the samples were tested for contact angle (5μL) of water and hexadecane and rolling angle (20μL of water, 10μL of hexadecane), and the liquid repellency performance data are shown in Table 3. All embodiments and comparative example 2 showed good liquid repellency; comparative example 3 had a certain contact angle for hexadecane, but when the substrate was tilted, the droplets could not slide down without a trace, and there was a serious droplet tailing phenomenon. The main reason for this phenomenon is that the surface of the former contains rich flexible -OS iO-PDMS segments, which is a typical liquid-like surface structure. Although the surface of comparative example 1 also contains rich flexible -OS iO-PDMS segments, its surface rough structure leads to an increase in static lipophilicity, and the rough structure leads to an increase in the sliding steric hindrance of the droplets, so that hexadecane cannot be removed; while the latter has no rich PDMS segments on the surface and contains more -CH3, showing extremely high lipophilicity.
[0085] In order to achieve an organic / inorganic ratio of less than 0.05 for the SiO2-like structure, a large proportion of oxygen and a higher plasma power were introduced during the deposition of the SiO2-like structure of Comparative Example 4, which intensified the oxidation of the particles during the deposition process to produce particles with higher affinity. These particles attracted each other to form dust and then dust particles, which were easily adsorbed on the substrate, resulting in a large number of adsorbed particles on the coating, forming super-hydrophobicity. Since the particles are not chemically bonded to the surface, they are easily destroyed, and water droplets will produce a pinning effect; and the lipophilic group of -CH3 provided in step S5 also causes the hexadecane to completely wet its surface and cannot be removed.
[0086] Table 3 Liquid repellency properties of all samples
[0087]
[0088]
[0089] As shown in Table 4, the pencil hardness of Examples 1-3 can reach 4H, which is greatly improved compared with Comparative Example 2. The reason for this phenomenon is that the addition of the cross-linked SiO2-like layer in the middle of the examples greatly improves the hardness of the coating. Compared with Comparative Example 5, the organic / inorganic component of the SiO2-like structure in Comparative Example 5 is greater than 0.3, the cross-linking degree is reduced, and the hardness of the coating decreases.
[0090] Table 4 Pencil hardness of Examples 1 to 3, Comparative Example 2, and Comparative Example 5
[0091] Example 1 Example 2 Example 3 Comparative Example 2 Comparative Example 5 Pencil hardness 4H 4H 4H 3B 1B
[0092] like Figure 6 As shown, after the cotton cloth wear test of Example 1 and Comparative Examples 5, 7 and 8, since the organic / inorganic component of the SiO2-like structure in Comparative Example 5 is greater than 0.3, the overall mechanical strength and mechanical durability of the coating are reduced; the organic / inorganic component of the PDMS-like structure in Comparative Example 7 is greater than 3, and the excessively long PDMS chain segments cause it to break very easily in the friction test, resulting in surface chemical heterogeneity, which affects the dynamic liquid-repellent performance of the coating. Figure 7 The XPS in-depth element analysis of the sample of Example 1 shows that Example 1 has a good gradient structure. Since there is no gradient structure between the SiO2-like structure and the PDMS-like structure in Comparative Example 8, PDMS bonds are easily broken during the friction process in Comparative Example 8.
[0093] Figures 8 to 10 The self-cleaning performance of Example 2 on different substrates and the effect of repelling oil in daily life are demonstrated, showing good liquid-repellent and anti-fouling properties.
[0094] In summary, the present application uses the PECVD method to prepare a thickness-controllable nano-gradient gradient durable liquid-like coating with cross-linked SiO2 and linear PDMS in a single step. It has good liquid-repellent and anti-fouling properties, a water contact angle of about 108° and an oil rolling angle of less than 10°. The film-base bonding grade of the coating is 5B, the pencil hardness can reach 4H, and the hardness can reach 1GPa. The high roughness of the coating prepared by plasma polymerization of siloxane monomers with a ring structure is effectively improved by means of a transition layer, so that the surface roughness of the coating is less than 1nm, giving a higher light transmittance. The nano-gradient structure is prepared by a continuous gradient gradient method, which effectively improves the durability of the prepared liquid-like coating.
[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A transparent fluorine-free liquid-repellent antifouling coating, It is characterized in that The antifouling coating comprises a transition layer, a SiO 2 The transition layer adopts an organic coating with different structural main chains according to different plating substrates; the SiO 2 The structure is the main part of the antifouling coating, wherein the organic / inorganic structure accounts for 0.05 to 0.3, and the silicon / oxygen element ratio is between 0.28 and 0.38; the PDMS-like structure includes periodic Si(CH 3 ) 2 Repeating units, wherein the organic / inorganic structure ratio is between 0.4 and 3.0, and the silicon / oxygen element ratio is between 0.4 and 0.
7.
2. The transparent fluorine-free liquid-repellent antifouling coating according to claim 1, It is characterized in that The plated substrate is an inorganic material or an organic material, the inorganic material is selected from glass, ceramic, stainless steel, copper, aluminum, and iron, and the organic material is selected from polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC), acrylonitrile-butadiene-styrene (ABS), polystyrene (PS), polycarbonate (PC), polyurethane (PU), rubber, natural polymer or PMMA; When the plating substrate is an inorganic material, the transition layer is an organic silicon coating with Si and O as the main chain; When the plating substrate is made of an organic material, the transition layer is an organic coating with a CC chain as the main chain.
3. The transparent fluorine-free liquid-repellent antifouling coating according to claim 1, It is characterized in that The inner structure of the antifouling coating changes from the smooth plasma polymer coating of the transition layer to the SiO-like 2 The structure then gradually transforms into a PDMS-like structure.
4. The transparent fluorine-free liquid-repellent antifouling coating according to claim 1, It is characterized in that The SiO-like 2 Si-(O) in the structure 3 and Si-(O) 4 The proportion is between 70% and 95%.
5. The transparent fluorine-free liquid-repellent antifouling coating according to claim 1, It is characterized in that The organic / inorganic structure ratio is the ratio of the silicon bonding in the characterization test. Compare.
6. The transparent fluorine-free liquid-repellent antifouling coating according to claim 1, It is characterized in that The transition layer, SiO 2 Both structures and PDMS-like structures are prepared continuously by a vapor phase method.
7. A method for preparing a transparent fluorine-free liquid-repellent antifouling coating according to any one of claims 1 to 6, It is characterized in that The steps include: S1: After cleaning and drying, the substrate is placed in a plasma chamber, and then the chamber is closed and vacuumed; S2: introducing activation gas, inputting plasma, cleaning and activating the surface of the substrate again, and increasing the surface temperature of the substrate, and then turning off the plasma and exhausting the additional gas; S3: introducing precursor A and auxiliary reaction gas D, inputting plasma, and completing the deposition of plasma polymer transition layer; S4: Adjust the plasma power and deposition pressure, input the precursor B and auxiliary reaction gas E for deposition at the same time, then turn off the auxiliary reaction gas D and precursor A in turn to complete the cross-linked SiO 2 Deposition of layers; S5: adjusting the deposition pressure, introducing the precursor C, depositing for several minutes, turning off the precursor B, adjusting the plasma power, depositing for several minutes, turning off the plasma input and all monomer inputs, exhausting the exhaust gas, breaking the vacuum, and then completing the preparation of the linear PDMS-like layer with a structural gradient; The deposition process from step S3 to step S5 is continuous and uninterrupted.
8. The method for preparing the transparent fluorine-free liquid-repellent antifouling coating according to claim 7, Features: The precursor A comprises one or a mixture of two or more of a linear hydrocarbon and a linear organosilane system, and the saturated vapor pressure is not less than 2.5 kPa at 20° C., including but not limited to the following monomers: tetraethyl orthosilicate, pentamethyldisiloxane, hexamethyldisiloxane, hexamethyldisilazane, bistrimethylsiloxymethylsilane, octamethyltrisiloxane, 1,1,3,3-tetramethyldisiloxane, tetramethyldivinyldisiloxane, vinylpentamethyldisiloxane, dimethoxymethylvinylsilane, 1,3-diethyl-1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-divinyl-hexamethyltrisiloxane, 1-vinyl-1,1,3,3-tetramethyldisiloxane, silane, methane, ethane, hexafluoropropylene, hexafluorobutyl acrylate, acrylic acid, butyl methacrylate; The precursor B is one or a mixture of two or more organic silane monomers having one or two or more rings, the relative silicon content in the precursor B is greater than 40%, and the saturated vapor pressure is not less than 0.1 kPa at 20° C., including but not limited to the following monomers: 2,4,6-trivinyl-2,4,6-trimethylcyclotrisiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, octamethylcyclotetrasiloxane, 2,4,6,8-tetramethyltetravinylcyclotetrasiloxane, heptamethylcyclotetrasiloxane, 2,4,6,8,10-cyclopentasiloxane, acetoxyheptamethylcyclotetrasiloxane; The precursor C is a linear organic silicon monomer with a main chain of -Si-O-, including but not limited to the following monomers: pentamethyldisiloxane, hexamethyldisiloxane, bistrimethylsiloxymethylsilane, octamethyltrisiloxane, 1,1,3,3-tetramethyldisiloxane, tetramethyldivinyldisiloxane, vinylpentamethyldisiloxane, 1,3-diethyl-1,1,3,3-tetramethyldisiloxane, 1-allyl-1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-divinyl-hexamethyltrisiloxane, 1-vinyl-1,1,3,3-tetramethyldisiloxane, 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane.
9. The method for preparing the transparent fluorine-free liquid-repellent antifouling coating according to claim 7, Features: The auxiliary reaction gases D and E are Ar, O 2 、N 2 , H 2 O, H 2 O 2 , H 2 One or a mixture of two or more.
10. The method for preparing the transparent fluorine-free liquid-repellent antifouling coating according to claim 7, Features: The time interval from closing the auxiliary reaction gas D and opening the precursor C to closing the precursor B is 10 to 300 seconds, and the deposition time from closing the precursor B to the end of deposition is 60 to 900 seconds.
Citation Information
Patent Citations
Superhydrophobic transparent waterproof membrane and preparation method thereof
CN109535785A
Protective coating
CN110268810A
Long-acting firm super-hydrophobic nano gradient composite coating and preparation method thereof
CN117259164A
Multi-layer coatings
US20160002498A1
Abrasion-resistant plastic articles and method for making them
US4927704A