Ultrahigh-temperature super-elastic thermal protection coating
Patent Information
- Application Number
- CN202410951646.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
但是随着温度和厚度的增加,TBC往往会出现以下问题:陶瓷层和粘结层界面容易出现脱落;陶瓷层在高温下内部产生微裂纹;涂层更易失效等问题
[0019] The present invention at least includes the following beneficial effects: The present invention utilizes spherical thin-walled empty shell nanometer t'-YSZ powder and Zr 0.84-x Y x Ce 0.16 O 2-0.5x Powder, an ultra-high temperature super-elastic thermal protective coating is prepared through atmospheric plasma spraying technology. The bonding layer powder and the first ceramic layer powder are mixed in a certain proportion to prepare a composite intermediate layer, which is located between the bonding layer and the ceramic layer, which can effectively improve the mismatch of thermal expansion coefficients between the ceramic layer and the bonding layer; the introduced The second ceramic layer is Zr 0.84- x Y x Ce 0.16 O 2-0.5x Prepared from powder materials, it has high toughness and low thermal conductivity, which can enhance the thermal insulation ability of the coating, eliminate the internal stress of the coating, and extend the life of the coating. By introducing a composite intermediate layer and two ceramic layers, the present invention effectively improves the interface bonding of the coating, increases its interface bonding ability, and improves the toughness, thermal shock resistance and heat insulation capabilities of the coating. The ultra-high-temperature super-elastic thermal protective coating of the present invention was subjected to 23 thermal shock cycles under ultra-high temperature (1750°C) conditions, and the coating remained intact without falling off. At the same time, its heat insulation capability (temperature difference between the coating surface and the back side) at 1500°C ≥900℃.
Smart Images

Figure CN118909477A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermal protection coatings, and more specifically, the present invention relates to an ultra-high temperature and ultra-elastic thermal protection coating. Background Art
[0002] With the rapid development of the aerospace industry, the development of ultra-high-speed aircraft has put forward higher requirements for engines. Engines need to have higher efficiency and withstand higher temperatures. Traditional YSZ will undergo coating sintering and phase change at 1200°C and cannot be used for a long time at this temperature (MRS Bulletin, 2012, 37(10): 891-943). Studies have shown that increasing the thickness of the YSZ ceramic layer can improve its thermal insulation capacity (~1K / μm, Surf. Coat. Technol., 205[5]1250-55(2010)). When the thickness of YSZ increases to 1000μm, the thermal insulation capacity can reach 1000K, which can meet the thermal insulation temperature requirements of the combustion chamber. However, with the increase of temperature and thickness, TBC often has the following problems: the interface between the ceramic layer and the bonding layer is prone to fall off; microcracks are generated inside the ceramic layer at high temperature; the coating is more likely to fail.
[0003] Material toughness is one of the key factors to improve the life of thick coatings. The fracture toughness (45J / m 2 ) is not enough to resist the thermal stress under extreme external environment. Therefore, developing materials with higher toughness is an effective measure to solve the current problem. In 2013, a paper in Science reported a small-sized Ce and Y-stabilized ZrO2 material with superelastic properties (DOI: 10.1126 / science.1239745). Its superelastic toughening mechanism (stress-induced martensitic phase transformation) is different from 7YSZ (ferroelastic toughening). Its toughness is comparable to that of shape memory alloys, and it is expected to solve the problem of insufficient toughness of YSZ thick coatings. So far, although there have been many reports on superelastic materials, there are no relevant literature reports on superelastic coatings.
[0004] The Zr 0.84-x Y x Ce 0.16 O 2-0.5xThe powder was used to prepare a 200μm double-layer superelastic coating (SC) (Chinese patent CN114480999B). The present invention uses atmospheric plasma spraying technology to prepare a four-layer structure (1000-1200μm thick) superelastic coating (NiCrAlY layer, NiCrAlY-YSZ layer, YSZ layer, SC layer). Among them, the NiCrAlY-YSZ layer effectively improves the YSZ / NiCrAlY interface bonding strength and alleviates the difference in thermal expansion coefficient of the YSZ / NiCrAlY interface; the SC layer acts as a thermal shock strain absorption layer, while improving the high temperature resistance and heat insulation capabilities of the coating. Summary of the invention
[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0006] In order to achieve these objects and other advantages of the present invention, an ultra-high temperature and ultra-elastic thermal protective coating is provided, comprising: a bonding layer prepared on a substrate, a composite intermediate layer prepared on the bonding layer, a first ceramic layer prepared on the composite intermediate layer, and a second ceramic layer prepared on the first ceramic layer;
[0007] The first ceramic layer powder used in the first ceramic layer is spherical thin-walled hollow shell nano t′-YSZ powder; the second ceramic layer powder used in the second ceramic layer is Zr 0.84-x Y x Ce 0.16 O 2-0.5x Powder, wherein x=0 to 0.02.
[0008] Preferably, the bonding layer is prepared by spraying bonding layer powder on the substrate using a supersonic flame spraying process, and the thickness of the bonding layer is 100-150 μm.
[0009] Preferably, the bonding layer powder is Oerlikon Metco Amdry 962 grade NiCrAlY, whose composition is Ni22Cr10Al1.0Y; and the matrix is GH5188 alloy.
[0010] Preferably, the composite intermediate layer is prepared by spraying composite intermediate layer powder on the bonding layer using an atmospheric plasma spraying process, and has a thickness of 100 to 150 μm.
[0011] Preferably, the composite intermediate layer powder is obtained by mixing the bonding layer powder and the first ceramic layer powder in a mass ratio of 1:1 to 5.
[0012] Preferably, the first ceramic layer is prepared by spraying the first ceramic layer powder on the composite intermediate layer using an atmospheric plasma spraying process, and the thickness of the first ceramic layer is 100 μm.
[0013] Preferably, the second ceramic layer is prepared by spraying the second ceramic layer powder on the first ceramic layer using an atmospheric plasma spraying process, and the thickness of the second ceramic layer is 700-800 μm.
[0014] Preferably, the process parameters of the atmospheric plasma spraying are: current 500-700A, voltage 60-80V, argon flow rate 60-130 liters / minute, hydrogen flow rate 12-22 liters / minute, spraying distance 80-130mm, powder feeding rate 30-45g / min, and gun speed 300-500mm / s.
[0015] Preferably, the composite intermediate layer powder is pretreated before use, and the specific method of the composite intermediate layer powder pretreatment is: NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder are mixed, added into a 1-5wt% polyvinyl pyrrolidone aqueous solution, stirred evenly, and the obtained mixed solution is subjected to high-frequency electromagnetic oscillation treatment, spray-dried at 250-350° C., and then heat-treated to obtain a pretreated composite intermediate layer powder;
[0016] Preferably, the ratio of the total mass of NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder to the volume of the polyvinyl pyrrolidone aqueous solution is 1g:10-50mL; the wavelength of the high-frequency electromagnetic oscillation treatment is 10-20mm, the frequency is 1000-2000MHz, and the treatment time is 10-15min; the specific method of heat treatment is: heating to 350-450°C at a heating rate of 5-10°C / min, keeping warm for 1-2h, then heating to 500-600°C at a heating rate of 5-10°C / min, keeping warm for 1-2h, and naturally cooling to room temperature.
[0017] Preferably, the ultra-high temperature and ultra-elastic thermal protective coating can be used at an ultra-high temperature of 1750°C.
[0018] Preferably, the ultra-high temperature and super-elastic thermal protective coating has a heat insulation capacity of ≥ 900°C at 1500°C.
[0019] The present invention at least has the following beneficial effects: the present invention utilizes spherical thin-walled hollow shell nano t′-YSZ powder and Zr 0.84-x Y x Ce 0.16 O 2-0.5x Powder, through atmospheric plasma spraying technology to prepare a super-high temperature super-elastic thermal protective coating. The bonding layer powder and the first ceramic layer powder are mixed in a certain proportion to prepare a composite intermediate layer, which is located between the bonding layer and the ceramic layer, and can effectively improve the thermal expansion coefficient mismatch problem between the ceramic layer and the bonding layer; the second ceramic layer introduced is Zr 0.84- x Y x Ce0.16 O 2-0.5x The powder material has high toughness and low thermal conductivity, which can enhance the thermal insulation ability of the coating, eliminate the internal stress of the coating, and extend the life of the coating. The present invention effectively improves the interface bonding of the coating by introducing a composite intermediate layer and two ceramic layers, increases its interface bonding ability, and improves the toughness, thermal shock resistance and thermal insulation of the coating. The ultra-high temperature and ultra-elastic thermal protective coating of the present invention has been subjected to 23 cycles of thermal shock under ultra-high temperature (1750°C) conditions, and the coating is intact without falling off. At the same time, at 1500°C, the thermal insulation ability (temperature difference between the surface and back of the coating) is ≥900°C.
[0020] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM image of the ultra-high temperature superelastic thermal protective coating prepared in Example 1;
[0022] Figure 2 This is the XRD pattern of the ultra-high temperature superelastic thermal protective coating prepared in Example 1;
[0023] Figure 3 This is the thermal shock heating curve of the ultra-high temperature superelastic thermal protective coating prepared in Example 1;
[0024] Figure 4 This is a photo of the ultra-high temperature superelastic thermal protective coating prepared in Example 1 after 23 cycles of thermal shock;
[0025] Figure 5 This is the XRD pattern of the ultra-high temperature superelastic thermal protective coating prepared in Example 1 after 23 cycles of thermal shock;
[0026] Figure 6 This is a SEM image of the thermal protection coating prepared in Comparative Example 2;
[0027] Figure 7 This is a comparison chart of the thermal insulation capabilities of the ultra-high temperature and super-elastic thermal protection coating prepared in Example 1 and the thermal protection coating prepared in Comparative Example 1 at 1200° C.;
[0028] Figure 8 This is a comparison chart of the thermal insulation capabilities of the ultra-high temperature superelastic thermal protection coating prepared in Example 1 and the thermal protection coating prepared in Comparative Example 1 at 1300° C.;
[0029] Fig. 9 This is a comparison chart of the thermal insulation capabilities of the ultra-high temperature superelastic thermal protection coating prepared in Example 1 and the thermal protection coating prepared in Comparative Example 1 at 1400°C;
[0030] Fig.10This is a comparison chart of the thermal insulation capabilities of the ultra-high temperature and super-elastic thermal protection coating prepared in Example 1 and the thermal protection coating prepared in Comparative Example 1 at 1500° C.;
[0031] Fig.11 The thermal shock temperature rise curve of the thermal protection coating prepared in Comparative Example 2;
[0032] Fig.12 This is a photo of the ultra-high temperature superelastic thermal protective coating prepared in Example 2 after 25 cycles of thermal shock;
[0033] Fig.13 It is a schematic diagram of the structure of the ultra-high temperature superelastic thermal protective coating of the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0035] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0036] In the following examples, the spherical thin-walled hollow shell nano t′-YSZ powder used was prepared by the preparation method described in patent CN114231886B; the Zr used 0.83 Y 0.01 Ce 0.16 The O2 powder is prepared by the preparation method described in patent CN114480999B.
[0037] Example 1
[0038] An ultra-high temperature and ultra-elastic thermal protective coating, such as Fig.13 As shown, including:
[0039] Bonding layer: The bonding layer powder is sprayed on the substrate GH5188 alloy by the supersonic flame spraying (HVOF) process, and its thickness is 100 μm; wherein, the substrate needs to remove surface oxides and oil stains before use, and then sandblasted; the bonding layer powder is Oerlikon Metco Amdry 962 NiCrAlY, and its specific parameters are shown in Table 1; the specific composition of the substrate GH5188 alloy is shown in Table 2.
[0040] Table 1
[0041] Brand Element Particle size distribution (μm) Applicable temperature (following spraying method) Amdry962 Ni22Cr10Al1.0Y 53~106 ≤980℃(APS) / ≤1050℃(HVOF)
[0042] Table 2
[0043]
[0044] Composite intermediate layer: The composite intermediate layer powder is sprayed on the bonding layer by atmospheric plasma spraying (APS) process, and the thickness is 100 μm; wherein the composite intermediate layer powder is a mixed powder obtained by mixing NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder in a mass ratio of 1:3, and the atmospheric plasma spraying process parameters are shown in Table 3;
[0045] The first ceramic layer (YSZ layer) is prepared by spraying the first ceramic layer powder on the composite intermediate layer by an atmospheric plasma spraying process, and the thickness is 100 μm; wherein the first ceramic layer powder is a spherical thin-walled hollow shell nano t′-YSZ powder, and the atmospheric plasma spraying process parameters are shown in Table 4;
[0046] The second ceramic layer (SC layer) is prepared by spraying the second ceramic layer powder on the first ceramic layer using an atmospheric plasma spraying process, with a thickness of 700 μm; wherein the second ceramic layer powder is Zr 0.83 Y 0.01 Ce 0.16 O2 powder, atmospheric plasma spraying process parameters are shown in Table 5.
[0047] The ultra-high temperature and ultra-elastic thermal protective coating prepared in this embodiment has a thickness of 1000 μm, wherein the thickness of the ceramic layer (the first ceramic layer and the second ceramic layer) is 800 μm.
[0048] Table 3
[0049]
[0050]
[0051] Table 4
[0052]
[0053] Table 5
[0054]
[0055] The microstructure of the ultra-high temperature superelastic thermal protective coating prepared in this embodiment was observed using a scanning electron microscope of model Ultra 55 produced by Zeiss, Germany, in backscattering mode. Figure 1 As shown, it can be seen that the interfaces between the YSZ layer and the composite interlayer, and between the composite interlayer and the bonding layer are clear and well bonded; there are evenly distributed voids inside the YSZ layer and the SC layer. The porosity of the SC layer is ~8%, and the porosity of the YSZ layer is ~8% as determined by Image J software.
[0056] The X′Pert PRO X-ray powder diffractometer produced by PANalytical of the Netherlands was used, and the main test parameters were: range scan 2θ = 10°-90°, step length 0.25°, high voltage maximum power 3kW, to determine whether there is an m phase; secondly, range scan 2θ = 72°-76°, step length 0.01°, to determine whether there is a c phase. Figure 2 As shown, the ultra-high temperature superelastic thermal protective coating prepared in Example 1 was analyzed, and the XRD test results of the deposited state obtained showed that the strongest peak was found at 30°, and double peaks were found at 71-75°. The main diffraction peak was attributed to the (111) interface of t′-YSZ, and the two diffraction peaks were attributed to the (004) and (400) crystal planes of t′-YSZ. Using the main diffraction peak near 30°, the Scherrer formula calculated the original powder grain size to be 36nm.
[0057] Gas thermal shock cycle experiment: The instrument used is the DWRZ03 thermal shock tester produced by Shaanxi Dewei Automation Co., Ltd. The thermal shock tester uses propane as fuel, oxygen as combustion aid, and cooling gas for temperature control. Propane is pressurized and atomized by high-pressure inert gas and pre-mixed with oxygen in the mixing chamber. Finally, the mixed gas enters the combustion chamber for combustion, and high-temperature and high-speed gas is sprayed out through a supersonic gas spray gun. The temperature is controlled by controlling the oxygen and propane gas content and the cooling gas flow rate. A high-temperature radiation thermometer is used to measure the surface temperature of the coating, as shown in Table 6. The oxygen and propane gas parameters are adjusted, the cooling gas flow rate is adjusted, the constant temperature is 1750℃, the heating time is 100s, the constant temperature time is 300s, and the cooling gas is used to cool the impacted coating for 400s before thermal shock, and so on.
[0058] Table 6
[0059] Temperature / ℃ Propane flow / SLM Oxygen flow / SLM Cooling air flow H / h 1750 2.5 7.5 4300
[0060] The thermal shock heating curve of the ultra-high temperature superelastic thermal protective coating prepared in Example 1 is as follows: Figure 3 The image curve is always around 1750℃, and the curve with 23 thermal shock times is still consistent with the curve with 10 thermal shock times, indicating that the coating can still be used normally after 23 tests at 1750℃, and the coating has the advantage of being recyclable. In addition, Figure 4 As shown in the figure, after 23 cycles of thermal shock, the coating was relatively intact as a whole, without large-scale shedding, indicating that it has excellent thermal shock resistance and can be used under ultra-high temperature conditions of 1750°C.
[0061] Superelasticity is a reversible phase transition of materials. When a stress is applied to the tetragonal phase, after an initial linear elastic response, a critical stress is reached, causing the phase transition to the monoclinic phase. When the stress is unloaded, the monoclinic phase has a linear elastic response and returns to the tetragonal phase (martensitic phase transition) (Science 341, 1505 (2013); DOI: 10.1126 / science.1239745). The high-temperature phase t phase of ZrO2 is retained to room temperature due to the compressive stress of the particles during the sintering process. When the material is subjected to external stress, the compressive stress of ZrO2 is released, and a phase transition from t to m occurs, which induces microcracks in the aggregate, thereby absorbing the expansion capacity of the main crack and achieving the purpose of improving the fracture toughness of the material (Science and technology of zirconia (2nd ed), vol. 12. Columbus (OH): American Ceramic Society; 1983. p. 103–238). High toughness can not only relieve the thermal stress caused by thermal mismatch between ceramic coating and metal substrate, but also resist the generation and propagation of microcracks in the coating (MRS Bull. 37 (2012) 891–898). Figure 5 This is the XRD graph of the ultra-high temperature superelastic thermal protective coating prepared in Example 1 after 23 cycles of thermal shock. The deposited state (As-sprayed) is the initial state of the coating after spraying. From the XRD spectrum, we can see that the deposited state only contains the characteristic peak of the t phase. After 23 cycles at high temperature, the coating has not only the characteristic peak of the t phase, but also the characteristic peak of the m phase, which is derived from the stress-induced t→m phase transition, indicating that the ultra-high temperature superelastic thermal protective coating prepared by the present invention has superelastic properties.
[0062] Comparative Example 1
[0063] A thermal protective coating comprises: a bonding layer prepared on a substrate, a composite intermediate layer prepared on the bonding layer, and a ceramic layer prepared on the composite intermediate layer; wherein the ceramic layer has a thickness of 800 μm, and the ceramic layer powder is a spherical thin-walled hollow shell nano t′-YSZ powder; the remaining methods and parameters are the same as those in Example 1; the only difference between this comparative example and Example 1 is that the ceramic layer in this comparative example is only a YSZ layer.
[0064] Comparative Example 2
[0065] The ceramic layer powder of this comparative example is Zr 0.83 Y 0.01 Ce 0.16 O2 powder, and the rest is the same as that of Comparative Example 1; the difference between this comparative example and Example 1 is that the ceramic layer of this comparative example is only the SC layer, and its SEM image is as shown Figure 6 shown.
[0066] The ultra-high temperature superelastic thermal protective coating prepared in Example 1 and the thermal protective coating prepared in Comparative Example 1 were subjected to gas thermal shock experiments at different temperatures: a high temperature radiation thermometer was used to measure the surface temperature of the coating, a thermocouple was welded on the back of the coating, a temperature indicator was connected, and the parameters were adjusted (Table 7). The temperature was controlled at 1200°C, 1300°C, 1400°C, and 1500°C, the heating time was 100s, and the constant temperature time was 300s. After the experiment, the coating surface was intact; the thermocouple was an armored thermocouple produced by Ningbo Aoqi Instrument Complete Equipment Co., Ltd., model WRKK-191-INC600, specification
[0067] Table 7
[0068] Temperature / ℃ Propane flow / SLM Oxygen flow / SLM Cooling air flow H / h 1200 1.6 5 3500 1300 1.6 5 2400 1400 1.6 5 2400 1500 1.8 5.5 2800
[0069] The results are as follows Figures 7-10 As shown, under the condition of 1200°C, the insulation temperature of Comparative Example 1 (YSZ) is 458°C, and the insulation temperature of Example 1 (superelastic) is 740°C, which is 61% higher than that of Comparative Example 1; under the condition of 1300°C, the insulation temperature of Comparative Example 1 is 465°C, and the insulation temperature of Example 1 is 743°C, which is 60% higher than that of Comparative Example 1; under the condition of 1400°C, the insulation temperature of Comparative Example 1 is 419°C, and the insulation temperature of Example 1 is 698°C, which is 67% higher than that of Comparative Example 1; under the condition of 1500°C, the insulation temperature of Comparative Example 1 is 642°C, and the insulation temperature of Example 1 is 929°C, which is 45% higher than that of Comparative Example 1; it can be seen that the ultra-high temperature superelastic thermal protective coating prepared in Example 1 of the present invention has excellent thermal insulation capability.
[0070] The thermal protection coating prepared in Example 2 was subjected to a gas thermal shock cycle test. The experimental parameters are shown in Table 6. The thermal shock temperature rise curve is shown in Fig.11 As shown, the curve is always around 1750°C. After three cycles, the coating fails and falls off before the fourth test. The coating does not have the ability to be recycled and the ability to resist thermal shock.
[0071] Example 2
[0072] In this embodiment, the composite intermediate layer powder is pretreated before use, and the remaining steps are the same as those in Example 1; wherein, the specific method for pretreatment of the composite intermediate layer powder is: NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder are mixed in a mass ratio of 1:3, added to a 2wt% polyvinyl pyrrolidone aqueous solution, stirred evenly, and the obtained mixed solution is subjected to high-frequency electromagnetic oscillation treatment, spray-dried at 320°C, and then heat-treated to obtain a pretreated composite intermediate layer powder; wherein, the ratio of the total mass of NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder to the volume of the polyvinyl pyrrolidone aqueous solution is 1g:20mL; the wavelength of the high-frequency electromagnetic oscillation is 15mm, the frequency is 1500MHz, and the time is 12min; the specific method for heat treatment is: heating to 400°C at a heating rate of 8°C / min, keeping warm for 1h, then heating to 550°C at a heating rate of 8°C / min, keeping warm for 1.5h, and naturally cooling to room temperature.
[0073] This embodiment uses high-frequency electromagnetic oscillation to treat the composite intermediate layer powder, and uses polyvinyl pyrrolidone as an auxiliary agent, which is beneficial to the refinement and uniformity of the mixed powder, avoiding the agglomeration of the powder. The coating formed by the powder during spraying is more uniform, and the interface bonding ability with the bonding layer and the ceramic layer is better, the interface bonding is tighter, and the coating is less likely to fall off under high-temperature thermal shock. The ultra-high temperature super-elastic thermal protective coating prepared in Example 2 was subjected to a gas thermal shock cycle experiment. The experimental parameters are shown in Table 6. At 1750°C, after 25 cycles of thermal shock, as shown in Table 6, Fig.12 As shown, the coating is intact and has not fallen off. Compared with Example 1, the ultra-high temperature and super-elastic thermal protective coating prepared in Example 2 has better resistance to thermal shock.
[0074] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. An ultra-high temperature and ultra-elastic thermal protective coating, characterized in that: include: Preparing a bonding layer on a substrate, preparing a composite intermediate layer on the bonding layer, preparing a first ceramic layer on the composite intermediate layer, and preparing a second ceramic layer on the first ceramic layer; The first ceramic layer powder used in the first ceramic layer is spherical thin-walled hollow shell nano t′-YSZ powder; the second ceramic layer powder used in the second ceramic layer is Zr 0.84-x Y x Ce 0.16 O 2-0.5x Powder, wherein x=0 to 0.
02.
2. The ultra-high temperature and ultra-elastic thermal protective coating according to claim 1, characterized in that: The bonding layer is prepared by spraying bonding layer powder on the substrate using a supersonic flame spraying process, and the thickness of the bonding layer is 100-150 μm.
3. The ultra-high temperature and ultra-elastic thermal protective coating according to claim 2, characterized in that: The bonding layer powder is Oerlikon Metco Amdry 962 brand NiCrAlY, whose composition is Ni22Cr10Al1.0Y; the matrix is GH5188 alloy.
4. The ultra-high temperature and ultra-elastic thermal protective coating according to claim 2, characterized in that: The composite middle layer is prepared by spraying composite middle layer powder on the bonding layer using an atmospheric plasma spraying process, and the thickness thereof is 100-150 μm.
5. The ultra-high temperature and ultra-elastic thermal protective coating according to claim 4, characterized in that: The composite intermediate layer powder is obtained by mixing the bonding layer powder and the first ceramic layer powder in a mass ratio of 1:1 to 5.
6. The ultra-high temperature and ultra-elastic thermal protective coating according to claim 4, characterized in that: The first ceramic layer is prepared by spraying the first ceramic layer powder on the composite intermediate layer using an atmospheric plasma spraying process, and the thickness of the first ceramic layer is 100 μm.
7. The ultra-high temperature and ultra-elastic thermal protective coating according to claim 6, characterized in that: The second ceramic layer is prepared by spraying the second ceramic layer powder on the first ceramic layer using an atmospheric plasma spraying process, and the thickness of the second ceramic layer is 700-800 μm.
8. The ultra-high temperature and ultra-elastic thermal protective coating according to claim 7, characterized in that: The process parameters of the atmospheric plasma spraying are: current 500-700A, voltage 60-80V, argon flow rate 60-130L / min, hydrogen flow rate 12-22L / min, spraying distance 80-130mm, powder feeding rate 30-45g / min, and gun speed 300-500mm / s.
9. The ultra-high temperature and ultra-elastic thermal protective coating according to any one of claims 1 to 8, characterized in that: The ultra-high temperature and ultra-elastic thermal protective coating can be used at an ultra-high temperature of 1750°C.
10. The ultra-high temperature and ultra-elastic thermal protective coating according to any one of claims 1 to 8, characterized in that: The ultra-high temperature and ultra-elastic thermal protective coating has a heat insulation capacity of ≥900°C at 1500°C.
Citation Information
Patent Citations
Double-ceramic-layer structure 8YSZ thermal barrier coating and preparation method
CN109706418A
Thermal barrier coating with composite double-ceramic-layer structure and preparation method thereof
CN113388801A
High-temperature long-life YSZ coating and preparation method thereof
CN114231886A
Ultrahigh-temperature long-service-life thermal barrier coating material and preparation method of ultrahigh-temperature long-service-life thermal barrier coating
CN114480999A
High-bonding-strength ceramic thermal barrier coating on surface of aluminum alloy and preparation method of high-bonding-strength ceramic thermal barrier coating
CN117568732A