Preparation method of polymer microsphere composite proppant
By adding thermoplastic powder styrene butadiene rubber and polymer microsphere composite proppant that degrades chopped fibers into the polymerization system, the settlement and compressive resistance of existing proppants in hydraulic fracturing technology are solved, and better results are achieved The suspension and diversion performance improves the production capacity of oil and gas wells.
Patent Information
- Application Number
- CN202410956350.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing proppants have problems in hydraulic fracturing technology, such as fast settlement speed, poor compressive resistance, poor flow diversion ability and poor suspension performance, and cannot meet the requirements of high suspension performance and flow diversion ability.
The preparation method of polymer microsphere composite proppant is adopted. By adding thermoplastic powder styrene-butadiene rubber and degradable chopped fibers to the polymerization system, the compressive and suspension properties of the proppant are improved, and the reasonable combination of additive systems is carried out. Optimize particle size distribution and pass rate.
It significantly reduces the crushing rate of proppant, improves suspension performance and flow diversion ability, meets the requirements of high suspension performance and flow diversion performance, and improves the fracturing effect.
Smart Images

Figure CN118909612A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of proppants used in oil and gas development, in particular to a method for preparing a polymer microsphere composite proppant. Background Art
[0002] Hydraulic fracturing technology is one of the most successful core technologies for the development and application of tight gas reservoirs such as shale gas. It is widely used in oil and gas reservoir production increase and transformation. The physical and chemical properties of the proppant, which is the fracture support material, will directly affect its production increase and transformation effect. The proppant is added to the fracturing fluid and pumped to the appropriate position in the fracture of the reservoir. The proppant forms a filling layer in the fracture to keep the fracture open, thereby forming a high-permeability flow channel for oil and gas circulation, and changes the flow type of the fluid in the formation from radial flow to bilinear flow, breaking through the near-wellbore blockage and connecting natural fractures, thereby significantly improving the production capacity of oil and gas wells.
[0003] Currently, the commonly used hydraulic fracturing technologies are guar gum fracturing fluid system and slick water fracturing fluid system. However, the conventional guar gum fracturing fluid system has the disadvantages of serious damage to low permeability reservoirs caused by the residues produced during fracturing, complex fluid preparation and high cost. The slick water fracturing fluid has low viscosity and conventional proppants are easy to settle when transported by slick water, resulting in problems such as premature sand removal of the proppant and a short half-length of the effective fracture.
[0004] Conventional proppants include quartz sand, ceramsite and coated quartz sand, etc. The density of these proppants is usually above 1.8g / cm3, and the sedimentation speed in slippery water is fast, which cannot fully meet the requirements of the current mainstream fracturing technology for high suspension performance of proppants. In recent years, there have been many reports on improved proppants, but these proppants often have problems such as poor compressive resistance (high breakage rate), poor conductivity, and poor suspension performance. Therefore, it is urgent to develop a proppant that is not easy to break, has good conductivity, and excellent suspension performance. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a polymer microsphere composite proppant, which has the advantages of being not easy to break, having good conductivity, good suspension performance and low density, and solves the problem that conventional proppants include quartz sand, ceramsite and coated quartz sand, etc., and the density of such proppants is usually above 1.8g / cm3, and the sedimentation rate in slippery water is fast, which cannot fully meet the requirements of the current mainstream fracturing technology for high suspension performance of proppants. In recent years, there have been many reports on improved proppants, but such proppants often have the problems of poor compressive resistance, poor conductivity and poor suspension performance.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a polymer microsphere composite proppant, comprising the following steps:
[0007] Prepare the aqueous phase: put polyvinyl alcohol, calcium montmorillonite and water in a certain proportion into a stirring tank A, fully dissolve and stir evenly to serve as the aqueous phase for the reaction.
[0008] Styrene monomer and thermoplastic powdered styrene butadiene rubber are placed in a stirred tank B protected by nitrogen, heated to 70°C and stirred until the thermoplastic powdered styrene butadiene rubber is fully dissolved in styrene.
[0009] The material in the stirring tank B is cooled to below 40°C, and divinylbenzene and benzoyl peroxide are added in sequence at a stirring speed of 20-40 r / min and mixed evenly to form the oil phase of the reaction.
[0010] The material in the stirring kettle B is quickly transferred to the reactor A (the stirring of the reactor A is not turned on at this time), and then the stirring of the stirring kettle A is started at a speed of 60-90 r / min and the temperature is raised to 80°C for reaction for 15-20 minutes, and then the degradable chopped fibers are added, and then the temperature is raised to 85-90°C and the reaction is continued for 2-3 hours.
[0011] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0012] Preferably, the amount of polyvinyl alcohol used is 1.5% to 4% of the weight of the water used. The polyvinyl alcohol is used as a main dispersant, which is beneficial to the control of the final particle size of the proppant.
[0013] Preferably, the amount of the calcium-based montmorillonite is 0.2% to 0.4% by weight of the water used. The calcium-based montmorillonite has a special lamellar structure and is mainly used as a dispersant.
[0014] Preferably, the amount of styrene used is 15-30% by weight of the water used.
[0015] Preferably, the amount of divinylbenzene used is 10-25% of the weight of the styrene used. The divinylbenzene is used as a cross-linking agent in the polymerization system. The cross-linked material has higher heat resistance, but the cross-linking will also make the material brittle. Therefore, the polymer microspheres prepared by the common styrene-divinylbenzene system are often brittle and are particularly easy to break under the action of external forces.
[0016] Preferably, the amount of benzoyl peroxide used is 0.5-1.5% of the weight of the styrene used. Thermoplastic styrene-butadiene rubber is also known as styrene-butadiene-styrene triblock copolymer (SBS for short).
[0017] Preferably, the amount of the thermoplastic powdered styrene-butadiene rubber is 5-15% of the weight of the styrene used.
[0018] Preferably, the degradable chopped fibers are polylactic acid fibers, and the length of the degradable chopped fibers is 2 to 4 mm. The polylactic acid fibers are a type of degradable fiber with excellent comprehensive performance. In a high-temperature water environment underground, the polylactic acid fibers can be quickly liquefied and degraded.
[0019] Preferably, the amount of the degradable chopped fibers is 5-10% of the weight of styrene.
[0020] Preferably, the particle size of the calcium-based montmorillonite is 3000 to 5000 mesh.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The invention improves the compressive resistance of the proppant by adding thermoplastic powdered styrene-butadiene rubber into the polymerization system, and significantly reduces the crushing rate. Degradable fibers are added into the polymerization system, which not only improves the strength of the material, further reduces the crushing rate, but also enables the proppant to have excellent suspension performance; and because the fibers used are degradable, the flow conductivity of the proppant is also greatly improved. By adopting a reasonable combination of the auxiliary agent system, the prepared proppant has good uniformity of particle size distribution and high qualified rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the suspension evaluation device of the present invention and the proppant before and after adding water, stirring and suspending.
[0024] In the figure: 1. measuring cylinder; 2. proppant particles before adding water; 3. proppant particles after adding water, stirring and suspending; 4. glass rod; 5. clean water. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be particularly noted that: the stirred tank A used in the present invention has a volume of 20L and a model of Gx-220, the stirred tank B has a volume of 20L and a model of Gx-320, and in the heating and cooling processes of the embodiments of the present invention and the comparative examples, unless otherwise specified, the heating and cooling rates used are all 5°C / min; the polyvinyl alcohol model used in the present invention is NJ-1; the SBS model used in the present invention is 792E; the short-cut polylactic acid fibers of different lengths are model 6D; and the calcium-based montmorillonite (model 30C, hereinafter referred to as CMMT) of different particle sizes.
[0027] Particle size qualification rate determination method:
[0028] Pour 50g of the prepared proppant sample into the standard test sieve (in descending order of mesh size), and then put the test sieve on the vibrating sieve machine. After vibrating for 5 minutes, weigh the mass of each sieve and the sample on the chassis. The weight of the sample with a mesh size of 20 to 60 is calculated as m0, and the particle size qualification rate is calculated as follows:
[0029] Particle size qualification rate = (m0 / 50)*100%
[0030] Determination method of breakage rate:
[0031] Screen out the required proppant sample, use an electronic analytical balance to accurately weigh 2.00g of the sample, pour the weighed sample into the crushing mold, place the mold on the press table, set the pressure to 52MPa, and remove the load after 2 minutes of stable load; then pour the pressurized sample into the specified sieve and vibrate the sieve, accurately weigh the crushed particles in the bottom plate, repeat the operation twice, and take the average value. The proppant crushing rate calculation formula is as follows:
[0032] K=(m / 2.00)*100%
[0033] Where: m is the mass of the crushed sample
[0034] Conductivity test method:
[0035] The proppant was soaked in 120℃ hot water for 4 days to fully degrade the degradable components in the proppant (simulating the degradation of the degradable components of the proppant in the formation), and then the sample was subjected to a short-term conductivity test according to the my country's petroleum and natural gas industry standard "Test Method for Conductivity of Fracturing Proppants" (SY / T 6302-2019). The closing pressure was 20MPa; the test temperature was 60℃; the artificial core used had a Mohs hardness of 6, a Young's modulus of 11GPa, and a Poisson's ratio of 0.23; the sand concentration was 10% by volume, that is, 10 volumes of the tested fracturing proppant corresponded to 100 volumes of fracturing fluid.
[0036] The present invention uses suspension density to evaluate the suspension performance of the proppant. The closer the suspension density is to 0 (but < 0), the better the suspension performance of the proppant. The test method is as follows:
[0037] 1. Add 20g of proppant into a 200ml measuring cylinder;
[0038] 2. Add 150ml of water into the measuring cylinder;
[0039] 3. Insert the glass rod into the bottom of the measuring cylinder and stir the mixture of the self-suspending proppant and clean water clockwise or counterclockwise to make it mix evenly;
[0040] 4. After 1 minute, read the accumulated volume of the proppant in the measuring cylinder and record it as V. See the test diagram for details. Figure 1 .
[0041] Suspension density = 20 / V
[0042] Example 1
[0043] The polymer microsphere composite proppant is prepared by the following steps:
[0044] Prepare the aqueous phase: put 230g of polyvinyl alcohol, 23g of calcium montmorillonite (3000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0045] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene-butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 30 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene-butadiene rubber in styrene.
[0046] The material in the stirring kettle B was cooled to 39°C, and 500 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 20 r / min and mixed evenly to serve as the oil phase of the reaction.
[0047] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 60 r / min and the temperature was raised to 80°C for reaction for 20 minutes. Then 100 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0048] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0049] Table 2 lists the test results of the proppant
[0050] Example 2
[0051] The polymer microsphere composite proppant is prepared by the following steps:
[0052] Prepare the aqueous phase: put 400g of polyvinyl alcohol, 20g of calcium-based montmorillonite (5000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0053] 2 kg of styrene monomer and 100 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0054] The material in the stirring tank B was cooled to 38°C, and 200 g of divinylbenzene and 30 g of benzoyl peroxide were added in sequence at a stirring speed of 40 r / min and mixed evenly to serve as the oil phase of the reaction.
[0055] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 60 r / min and the temperature was raised to 80°C for reaction for 15 minutes, and then 200 g of 2 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 85°C and the reaction was continued for 3 hours.
[0056] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0057] Table 2 lists the test results of the proppant
[0058] Example 3
[0059] The polymer microsphere composite proppant is prepared by the following steps:
[0060] Prepare the aqueous phase: put 250g of polyvinyl alcohol, 40g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0061] 2 kg of styrene monomer and 300 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0062] The material in the stirring kettle B was cooled to 40°C, and 400 g of divinylbenzene and 10 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0063] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 90 r / min and the temperature was raised to 80°C for reaction for 20 minutes. Then 150 g of 4 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2.5 hours.
[0064] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0065] Table 2 lists the test results of the proppant
[0066] Example 4
[0067] The polymer microsphere composite proppant is prepared by the following steps:
[0068] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0069] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0070] The material in the stirring tank B was cooled to 39°C, and 300 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0071] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 70 r / min and the temperature was raised to 80°C for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0072] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0073] Table 2 lists the test results of the proppant
[0074] Example 5
[0075] The polymer microsphere composite proppant is prepared by the following steps:
[0076] Prepare the aqueous phase: put 150g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir evenly, which serves as the aqueous phase for the reaction.
[0077] 1 kg of styrene monomer and 100 g of thermoplastic powdered styrene-butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene-butadiene rubber in styrene.
[0078] The material in the stirring tank B was cooled to 39°C, and 150 g of divinylbenzene and 12 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0079] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 75 r / min and the temperature was raised to 80°C for 18 minutes. Then 80 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 88°C and the reaction was continued for 2.5 hours.
[0080] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0081] Table 2 lists the test results of the proppant
[0082] Example 6
[0083] The polymer microsphere composite proppant is prepared by the following steps:
[0084] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0085] 2.5 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0086] The material in the stirring tank B was cooled to 39°C, and 300 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0087] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 80 r / min and the temperature was raised to 80°C for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0088] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0089] Table 2 lists the test results of the proppant
[0090] Example 7
[0091] The polymer microsphere composite proppant is prepared by the following steps:
[0092] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 35g of calcium-based montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0093] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0094] The material in the stirring tank B was cooled to 39°C, and 250 g of divinylbenzene and 18 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0095] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 80 r / min and the temperature was raised to 80°C for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0096] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0097] Table 2 lists the test results of the proppant
[0098] Example 8
[0099] The polymer microsphere composite proppant is prepared by the following steps:
[0100] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0101] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0102] The material in the stirring tank B was cooled to 39°C, and 300 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0103] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 80 r / min and the temperature was raised to 80°C for reaction for 18 minutes, and then 180 g of 4 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 88°C and the reaction was continued for 2.5 hours.
[0104] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0105] Table 2 lists the test results of the proppant
[0106] Example 9
[0107] The polymer microsphere composite proppant is prepared by the following steps:
[0108] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0109] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0110] The material in the stirring tank B was cooled to 39°C, and 450 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0111] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 80 r / min and the temperature was raised to 80°C for reaction for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 88°C and the reaction was continued for 2.5 hours.
[0112] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0113] Table 2 lists the test results of the proppant
[0114] Comparative Example 1
[0115] The addition time period of the polylactic acid fiber was adjusted, and the remaining operations were the same as those in Example 4. The polymer microsphere composite proppant was prepared by the following steps:
[0116] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0117] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0118] The material in the stirring tank B was cooled to 39°C, and the following were added in sequence at a stirring speed of 30 r / min: 300 g of divinylbenzene, 20 g of benzoyl peroxide, and 160 g of 3 mm long short-cut polylactic acid fibers. The mixture was mixed evenly to prepare the oil phase for the reaction.
[0119] The material in stirring kettle B was quickly transferred to reactor A (the stirring of reactor A was not turned on at this time), and then stirring was started in stirring kettle A at a speed of 70 r / min and the temperature was raised to 80°C for reaction for 18 minutes, and then the temperature was raised to 90°C for further reaction for 2 hours.
[0120] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0121] Comparative Example 2
[0122] Without adding thermoplastic powdered styrene-butadiene rubber (SBS), the remaining operations were the same as those in Example 4, and the polymer microsphere composite proppant was prepared by the following steps:
[0123] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0124] The material in the stirring tank B was cooled to 39°C, and 300 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0125] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 70 r / min and the temperature was raised to 80°C for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0126] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0127] Table 2 lists the test results of the proppant
[0128] Comparative Example 3
[0129] Without adding short-cut polylactic acid fibers, the remaining operations were the same as those in Example 4, and the polymer microsphere composite proppant was prepared by the following steps:
[0130] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0131] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0132] The material in the stirring tank B was cooled to 39°C, and 300 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0133] The material in stirring kettle B was quickly transferred to reactor A (the stirring of reactor A was not turned on at this time), and then stirring was started in stirring kettle A at a speed of 70 r / min and the temperature was raised to 80°C for reaction for 18 minutes, and then the temperature was raised to 90°C for further reaction for 2 hours.
[0134] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0135] Table 2 lists the test results of the proppant
[0136] Comparative Example 4
[0137] Without adding divinylbenzene, the remaining operations were the same as those in Example 4, and the polymer microsphere composite proppant was prepared by the following steps:
[0138] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (4000 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0139] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0140] The material in the stirring tank B was cooled to 39°C, and 20 g of benzoyl peroxide was added at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0141] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 70 r / min and the temperature was raised to 80°C for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0142] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0143] Table 2 lists the test results of the proppant
[0144] Comparative Example 5
[0145] The polymer microsphere composite proppant is prepared by the following steps:
[0146] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium phosphate (4000 mesh) and 10kg of water into a stirring tank A according to a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir evenly, which serves as the aqueous phase for the reaction.
[0147] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0148] The material in the stirring tank B was cooled to 39°C, and 300 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0149] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 70 r / min and the temperature was raised to 80°C for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0150] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0151] Table 2 lists the test results of the proppant
[0152] Comparative Example 6
[0153] The polymer microsphere composite proppant is prepared by the following steps:
[0154] Prepare the aqueous phase: put 300g of polyvinyl alcohol, 30g of calcium montmorillonite (1250 mesh) and 10kg of water into a stirring tank A in a certain proportion and stir at a stirring speed of 60r / min at room temperature for 1h to fully dissolve the materials and stir them evenly, which serves as the aqueous phase for the reaction.
[0155] 2 kg of styrene monomer and 200 g of thermoplastic powdered styrene butadiene rubber (SBS) were placed in a stirred tank B under nitrogen protection, heated to 70°C, stirred at a speed of 50 r / min, and stirred for 1 hour to fully dissolve the thermoplastic powdered styrene butadiene rubber in styrene.
[0156] The material in the stirring tank B was cooled to 39°C, and 300 g of divinylbenzene and 20 g of benzoyl peroxide were added in sequence at a stirring speed of 30 r / min and mixed evenly to serve as the oil phase of the reaction.
[0157] The material in the stirring kettle B was quickly transferred to the reactor A (the stirring of the reactor A was not turned on at this time), and then the stirring of the stirring kettle A was started at a speed of 70 r / min and the temperature was raised to 80°C for 18 minutes. Then 160 g of 3 mm long short-cut polylactic acid fibers were added, and then the temperature was raised to 90°C and the reaction was continued for 2 hours.
[0158] The polymer microsphere composite proppant is obtained after filtering, washing and drying.
[0159] Table 1 Material formula of the embodiment and comparative example
[0160]
[0161] Note: “0” means that the component is not added
[0162] Table 2 Proppant test results
[0163]
[0164] The standard parts used in this application document can all be purchased from the market and can be customized according to the description in the specification and drawings. The specific connection methods of each part adopt conventional means such as mature bolts, rivets, welding, etc. in the prior art. The machinery, parts and equipment all adopt conventional models in the prior art. The control method is automatic control through a controller. The control circuit of the controller can be implemented through simple programming by technicians in this field, which is common knowledge in the field. This application is mainly used to protect mechanical devices, so this application no longer explains the control method and circuit connection in detail.
[0165] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0166] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a polymer microsphere composite proppant, characterized in that: The steps include: Prepare the aqueous phase: put polyvinyl alcohol, calcium montmorillonite and water in a certain proportion into a stirring tank A, fully dissolve and stir evenly to serve as the aqueous phase for the reaction. Styrene monomer and thermoplastic powdered styrene butadiene rubber are placed in a stirred tank B protected by nitrogen, heated to 70°C and stirred until the thermoplastic powdered styrene butadiene rubber is fully dissolved in styrene. The material in the stirring tank B is cooled to below 40°C, and divinylbenzene and benzoyl peroxide are added in sequence at a stirring speed of 20-40 r / min and mixed evenly to form the oil phase of the reaction. The material in the stirring kettle B is quickly transferred to the reactor A (the stirring of the reactor A is not turned on at this time), and then the stirring of the stirring kettle A is started at a speed of 60-90 r / min and the temperature is raised to 80°C for reaction for 15-20 minutes, and then the degradable chopped fibers are added, and then the temperature is raised to 85-90°C and the reaction is continued for 2-3 hours. The polymer microsphere composite proppant is obtained after filtering, washing and drying.
2. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The amount of polyvinyl alcohol used is 1.5% to 4% of the weight of the water used.
3. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The amount of calcium-based montmorillonite used is 0.2% to 0.4% of the weight of the water used.
4. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The amount of styrene used is 15-30% of the weight of the water used.
5. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The amount of divinylbenzene used is 10-25% of the weight of the styrene used.
6. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The amount of benzoyl peroxide used is 0.5-1.5% of the weight of the styrene used.
7. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The amount of the thermoplastic powdered styrene-butadiene rubber used is 5-15% of the weight of the styrene used.
8. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The degradable chopped fibers are polylactic acid fibers, and the length of the degradable chopped fibers is 2 to 4 mm.
9. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The amount of the degradable chopped fibers is 5-10% of the weight of styrene.
10. The method for preparing a polymer microsphere composite proppant according to claim 1, characterized in that: The particle size of the calcium-based montmorillonite is 3000-5000 meshes.