Nanoparticles capable of emitting ultraviolet light and green light through near-infrared excitation orthogonal upconversion and preparation method and application thereof

Through the chemical composition and preparation method of β-NaYF4:Nd3+/Yb3+/Tm3+@β-NaYF4:Nd3+@β-NaYF4@NaYF4:Yb3+/Er3+ nanoparticles, the problem of orthogonal upconversion luminescence under near-infrared excitation is solved, and the problem of orthogonal upconversion luminescence under near-infrared excitation is realized. Efficient optical imaging and biomedical applications.

CN118909613APending Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410949389.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively realize the preparation of orthogonal upconversion nanoparticles that emit ultraviolet and green light under near-infrared band excitation, which limits the design and application of new optical devices.

Method used

The chemical composition of nanoparticles of β-NaYF4:Nd3+/Yb3+/Tm3+@β-NaYF4:Nd3+@β-NaYF4@NaYF4:Yb3+/Er3+ is used to utilize the interface energy transfer characteristics of Yb3+ and the doping of Nd3+. The cross-relaxation effect achieves upconversion luminescence under 808nm and 980nm near-infrared excitation, and combines a multifunctional red or green light emission layer and an inert protective layer to regulate the spectral response of nanoparticles.

Benefits of technology

Efficient orthogonal upconversion of ultraviolet and green light under near-infrared excitation is achieved, providing higher optical imaging resolution and biomedical imaging possibilities, avoiding damage and interference to biological tissues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909613A_ABST
    Figure CN118909613A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of luminescent materials, and discloses a nano particle capable of emitting ultraviolet light and green light through near-infrared excitation orthogonal upconversion and a preparation method and application thereof.The chemical composition of the nano particle is beta-NaYF4: Nd < 3 + > / Yb < 3 + > / Tm < 3 + > at-NaYF4: Nd < 3 + > at-NaYF4 at-NaYF4: Yb < 3 + > / Er < 3 + >, the nano particle is of a core-shell structure, and specifically, NaYF4 doped with an exciting agent Tm < 3 + > and a sensitizing agent Nd < 3 + > serves as an inner core, and NaYF4 doped with an exciting agent Nd < 3 + > serves as an outer core; er < 3 + > and Yb < 3 + > doped NaF4 is used as a shell, and Nd < 3 + > doped NaF4 is used as an optical inert layer and an inert isolation layer NaYF4 in the middle. By utilizing the interface energy transfer characteristic of Y < 3 + >, the cross relaxation between Yb < 3 + > and Tm < 3 + >, the cross relaxation between Yb < 3 + > and Er < 3 + > and the multifunctional effect of the first emission shell layer, the up-conversion orthogonal ultraviolet light and green light emitting nanoparticles which respond under the excitation of near-infrared wavelengths of 980nm and 808nm are realized; the medical value that low-energy high-transmission near-infrared rays penetrate through biological tissues to be converted into high-energy light in the biomedical neighborhood to drive molecular movement, control release and the like is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of luminescent materials, and in particular relates to a nanoparticle that emits ultraviolet light and green light by orthogonal up-conversion through near-infrared excitation, and a preparation method and application thereof. Background Art

[0002] In recent years, the rapid development of nanotechnology has brought new opportunities and challenges to the research and application of optics. In terms of optical materials and devices, people are paying more and more attention to the research and development of materials that can emit ultraviolet and green light under near-infrared excitation. Since such materials can not only effectively utilize the excitation energy in the near-infrared spectral range, but also have the ability to emit specific wavelengths of light in other wavelength ranges, they have important application potential.

[0003] In traditional fluorescent materials, ultraviolet or visible light is usually required for excitation, while near-infrared excitation has the advantages of strong penetration and tissue transparency, so it is considered to be a more attractive excitation method. The preparation method of nanoparticles that orthogonally upconvert ultraviolet and green light by near-infrared excitation can overcome some limitations of traditional methods and provide new ideas and approaches for the design and preparation of new optical devices.

[0004] Therefore, in order to overcome the limitations of traditional technologies, it is an urgent problem for technicians in this field to provide nanoparticles that emit ultraviolet and green light by orthogonal up-conversion under near-infrared excitation and a preparation method thereof. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a nanoparticle that emits ultraviolet light and green light by orthogonal up-conversion under near-infrared excitation, and a preparation method and application thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A nanoparticle that emits ultraviolet light and green light by orthogonal upconversion under near-infrared excitation, wherein the chemical composition of the nanoparticle is:

[0008] β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ .

[0009] In the chemical composition of the nanoparticles provided by the present invention, Tm 3+ Exists in the innermost shell as an activator, and the second and third shells are activated by Nd 3+ The doping shortens the Er 3+and Tm 3+ The luminescence lifetime, thus achieving upconversion nanoparticles requires high power density excitation at 808nm, rather than being excited by low-power 980nm near-infrared light to achieve better orthogonal upconversion.

[0010] At the same time, the present invention utilizes Y 3+ The interfacial energy transfer characteristics of Yb 3+ and Tm 3+ Yb 3+ and Er 3+ The cross-relaxation between the two and the multifunctional effect of the first emission shell (red light or green light emission layer and inert protective layer) realize the up-conversion of orthogonal ultraviolet and green light luminescent nanoparticles that respond under excitation of near-infrared wavelengths of 980nm and 808nm, realizing the medical value of low-energy and high-transmittance near-infrared in the biomedical field, which is converted into high-energy light when passing through biological tissues to drive molecular movement and control release.

[0011] Preferably, the nanoparticles are of core-shell structure, specifically doped with an activator Tm 3+ and sensitizer Nd 3+ NaYF4 is used as the core, doped with Er 3+ and Yb 3+ NaF4 is the outer shell, and Nd is in the middle. 3+ Doped NaF4 is an optically inert layer and an inert isolation layer NaYF4.

[0012] Preferably, the β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ Medium Nd 3+ The molar concentration is 0.5-1mol%, Yb 3+ The molar concentration is 20-30 mol%, Tm 3+ The molar concentration is 0.5 mol%;

[0013] The β-NaYF4:Nd 3+ Medium Nd 3+ The molar concentration is 20-30 mol%;

[0014] The NaYF4:Yb 3+ / Er 3+ Medium 3+ The molar concentration of Er is 18 mol%. 3+ The molar concentration is 2 mol%.

[0015] Preferably, the nanoparticles emit ultraviolet light when irradiated with near-infrared light with a wavelength of 980 nm as an excitation source, and emit blue-green light up-conversion spectrum when irradiated with near-infrared light with a wavelength of 808 nm as an excitation source.

[0016] Preferably, the nanoparticles are prepared by thermal decomposition.

[0017] According to the above-mentioned method for preparing near-infrared excited orthogonal up-conversion ultraviolet and green light emitting nanoparticles, the method comprises the following specific steps:

[0018] (1) Y(CH3CO2)3·xH2O, Nd(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Tm(CH3CO2)3·xH2O were mixed and reacted at a constant temperature in a mixed solution of oleic acid and 1-octadecene after vacuum evacuation to form a complex. After cooling to room temperature, a methanol solution of NH4F and NaOH was added to react under an argon atmosphere. Finally, ethanol was added to precipitate the core β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ Nanoparticles were dispersed in n-hexane to obtain the core rare earth complex precursor;

[0019] (2) Y(CH3CO2)3·xH2O and Nd(CH3CO2)3·xH2O are weighed, and after vacuuming in a mixed solution of oleic acid and 1-octadecene, the mixture is reacted at a constant temperature to form a complex, and then the nuclear rare earth complex precursor obtained in step (1) is added, and the n-hexane is removed by heating. After cooling to room temperature, a methanol solution of NH4F and NaOH is added, and the mixture is reacted under an argon environment to obtain β-NaYF4:Nd 3 + / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Nanoparticles were dispersed in n-hexane to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Nanoparticle dispersion;

[0020] (3) Y(CH3CO2)3·xH2O is weighed and subjected to constant temperature reaction in a mixed solution of oleic acid and 1-octadecene after vacuuming to form a complex, and then the β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+The nanoparticle dispersion was heated to remove n-hexane, and after cooling to room temperature, NH4F and NaOH methanol solution were added to react under argon environment to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticles are dispersed in n-hexane to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticle dispersion;

[0021] (4) Y(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Er(CH3CO2)3·xH2O are weighed, and a mixed solution of oleic acid and 1-octadecene is evacuated and reacted at a constant temperature to form a complex, and then the nanoparticle dispersion obtained in step (2) is added and heated to remove n-hexane. After cooling to room temperature, a methanol solution of NH4F and NaOH is added and reacted under an argon environment to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ Nanoparticles.

[0022] Preferably, the mass ratio of Y(CH3CO2)3·xH2O, Nd(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Tm(CH3CO2)3·xH2O in step (1) is 380-400:6-7:25-26:4-5;

[0023] The mass ratio of Y(CH3CO2)3·xH2O to Nd(CH3CO2)3·xH2O in step (2) is 380-420:72-75;

[0024] The mass ratio of Y(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Er(CH3CO2)3·xH2O in step (4) is 380-420:102-105:13-14;

[0025] The mass ratio of Y(CH3CO2)3·xH2O in steps (1), (2), (3) and (4) is 1:1:1:1.

[0026] Preferably, the isothermal reaction conditions in steps (1), (2), (3) and (4) are: reaction at 130° C. for 30-60 min;

[0027] The reaction under argon environment in steps (1), (2), (3) and (4) is as follows: after removing methanol, react at 300° C. for 60-90 minutes.

[0028] Application of the near-infrared excited orthogonal up-conversion nanoparticles emitting ultraviolet and green light as described above or the near-infrared excited orthogonal up-conversion nanoparticles emitting ultraviolet and green light obtained by the above preparation method in optical imaging technology and biomedicine.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention provides a nanoparticle that emits ultraviolet light and green light by orthogonal upconversion under near-infrared excitation, and a preparation method and application thereof. The nanomaterial of the present invention has special optical properties and surface effects, and its spectral response and fluorescence performance can be regulated, thereby achieving precise regulation of the performance of optical devices. By utilizing near-infrared excitation, deep imaging of biological tissues can be achieved, thereby avoiding damage and interference to the tissues.

[0031] At the same time, the nanomaterials of the present invention can obtain higher resolution and richer imaging information by emitting ultraviolet light and green light through orthogonal up-conversion, providing more possibilities for biomedical imaging. Moreover, by emitting ultraviolet light and green light through orthogonal up-conversion via near-infrared excitation, some molecules inside the tissue that receive ultraviolet light or blue-green light can be regulated to achieve long-distance regulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0033] Figure 1 The transmission electron microscope images of the nanoparticles in various processes during the preparation process of the embodiment of the present invention are shown;

[0034] Figure 2 The nanoparticles prepared in the embodiment of the present invention emit ultraviolet light under 980nm near-infrared light irradiation and the up-conversion spectrum of blue-green light under 808nm irradiation;

[0035] Figure 3 This is an XRD image of nanoparticles prepared according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] A method for preparing nanoparticles that emit ultraviolet light and green light by near-infrared excitation orthogonal upconversion comprises the following specific steps:

[0039] (1) Core β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ Synthesis of Nanoparticles:

[0040] 380 mg (CH3CO2)3·xH2O, 6 mg Nd(CH3CO2)3·xH2O, 25 mg Yb(CH3CO2)3·xH2O and 4 mg Tm(CH3CO2)3·xH2O were dissolved in 12 mL oleic acid and 15 mL 1-octadecene mixed solvent, and the mixture was heated and evacuated at 130°C for 30 min to form a lanthanide-oleate complex and remove moisture; then the solution was cooled to 50°C, argon was continuously passed, 10 mL methanol solution containing NH4F (8 mmol) and NaOH (200 mg) was added to the solution, and after stirring for 30 min, methanol was removed, and then the solution was heated to 300°C under argon for 90 min and cooled to room temperature; finally, 30 mL ethanol was added to precipitate the core β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ The nanoparticles were finally dispersed in 10 ml of n-hexane to obtain the core rare earth complex precursor;

[0041] (2) β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Synthesis of:

[0042] 380 mg Y(CH3CO2)3·xH2O and 72 mg Nd(CH3CO2)3·xH2O are added to a mixed solvent of 12 mL oleic acid and 15 mL 1-octadecene, and the mixture is heated at 130°C under vacuum for 30 min to form a lanthanum niobate complex and remove moisture; then the solution is cooled to 80°C in an argon atmosphere, and the nuclear rare earth complex precursor obtained in step (1) is added to the solution, heated to 90°C, and n-hexane is removed, and then the solution is cooled to 50°C, 10 mL methanol solution containing NH4F (8 mmol) and NaOH (200 mg) is added, and after stirring for 30 min, the methanol is removed, and then the solution is heated to 300°C under an argon atmosphere and left for 90 min; finally, the solution is cooled to room temperature, the solution is centrifuged, the solvent is removed, and then washed with ethanol several times to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3 + @β-NaYF4:Nd 3+ The nanoparticles were finally dispersed in 10 ml of n-hexane to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Nanoparticle dispersion;

[0043] (3) Core-shell (II) β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Synthesis of @β-NaYF4:

[0044] 380 mg of Y(CH3CO2)3·xH2O was added to a mixed solvent of 12 mL of oleic acid and 15 mL of 1-octadecene, and the mixture was heated at 130°C under vacuum for 30 min to form a lanthanum niobate complex and remove moisture; the solution was then cooled to 80°C in an argon atmosphere, and the β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ The nanoparticle dispersion was added to the solution, heated to 90 °C, the n-hexane was removed, and then the solution was cooled to 50 °C, 10 mL of methanol solution containing NH4F (8 mmol) and NaOH (200 mg) was added, and stirred for 30 min, then the methanol was removed, and then heated to 300 °C under an argon atmosphere for 90 min; finally, it was cooled to room temperature, the solution was centrifuged, the solvent was removed, and then washed with ethanol several times to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticles were finally dispersed in 10 ml of n-hexane to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticle dispersion;

[0045] (4) Core-shell (III) β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ Synthesis of:

[0046] 380 mg of Y(CH3CO2)3·xH2O, 102 mg of Yb(CH3CO2)3·xH2O and 13 mg of Er(CH3CO2)3·xH2O were added to a mixed solvent of 12 mL of oleic acid and 15 mL of 1-octadecene, and the mixture was heated at 130°C under vacuum for 30 min to form a lanthanum niobate complex and remove moisture; the solution was then cooled to 80°C in an argon atmosphere, and the β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticle dispersion was added to the solution, heated to 90°C, n-hexane was removed, and then the solution was cooled to 50°C, 10 mL of methanol solution containing NH4F (8 mmol) and NaOH (200 mg) was added, and stirred for 30 min, then methanol was removed, and then heated to 300°C under an argon atmosphere for 90 min; finally, cooled to room temperature, the solution was centrifuged to remove the solvent, and then washed with ethanol several times to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ Nanoparticles.

[0047] Example 2

[0048] A method for preparing nanoparticles that emit ultraviolet light and green light by near-infrared excitation orthogonal upconversion comprises the following specific steps:

[0049] (1) Core β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ Synthesis of Nanoparticles:

[0050] 400 mg (CH3CO2)3·xH2O, 7 mg Nd(CH3CO2)3·xH2O, 26 mg Yb(CH3CO2)3·xH2O and 5 mg Tm(CH3CO2)3·xH2O were dissolved in 12 mL oleic acid and 15 mL 1-octadecene mixed solvent, and the mixture was heated at 130°C and vacuumed for 30 min to form a lanthanide-oleate complex and remove moisture; then the solution was cooled to 50°C, argon was continuously passed, 10 mL methanol solution containing NH4F (8 mmol) and NaOH (200 mg) was added to the solution, and after stirring for 30 min, methanol was removed, and then the solution was heated to 300°C under argon for 90 min and cooled to room temperature; finally, 30 mL ethanol was added to precipitate the core β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ The nanoparticles were finally dispersed in 10 ml of n-hexane to obtain the core rare earth complex precursor;

[0051] (2) β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Synthesis of:

[0052] 420 mg of Y(CH3CO2)3·xH2O and 75 mg of Nd(CH3CO2)3·xH2O were added to a mixed solvent of 12 mL of oleic acid and 15 mL of 1-octadecene, and the mixture was heated at 130°C under vacuum for 30 min to form a lanthanum niobate complex and remove moisture; the solution was then cooled to 80°C in an argon atmosphere, and the nuclear rare earth complex precursor obtained in step (1) was added to the solution, heated to 90°C, and n-hexane was removed, and the solution was then cooled to 50°C, 10 mL of methanol solution containing NH4F (8 mmol) and NaOH (200 mg) was added, and stirred for 30 min, and then the methanol was removed, and then heated to 300°C in an argon atmosphere for 90 min; finally, cooled to room temperature, the solution was centrifuged, the solvent was removed, and then washed with ethanol several times to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3 + @β-NaYF4:Nd 3+ The nanoparticles were finally dispersed in 10 ml of n-hexane to obtain β-NaYF4:Nd 3+ / Yb3+ / Tm 3+ @β-NaYF4:Nd 3+ Nanoparticle dispersion;

[0053] (3) Core-shell (II) β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Synthesis of @β-NaYF4:

[0054] 420 mg of Y(CH3CO2)3·xH2O was added to a mixed solvent of 12 mL of oleic acid and 15 mL of 1-octadecene, and the mixture was heated at 130°C under vacuum for 30 min to form a lanthanum niobate complex and remove moisture; the solution was then cooled to 80°C in an argon atmosphere, and the β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ The nanoparticle dispersion was added to the solution, heated to 90 °C, the n-hexane was removed, and then the solution was cooled to 50 °C, 10 mL of methanol solution containing NH4F (8 mmol) and NaOH (200 mg) was added, and stirred for 30 min, then the methanol was removed, and then heated to 300 °C under an argon atmosphere for 90 min; finally, it was cooled to room temperature, the solution was centrifuged, the solvent was removed, and then washed with ethanol several times to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticles were finally dispersed in 10 ml of n-hexane to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticle dispersion;

[0055] (4) Core-shell (III) β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ Synthesis of:

[0056] 420 mg of Y(CH3CO2)3·xH2O, 105 mg of Yb(CH3CO2)3·xH2O and 14 mg of Er(CH3CO2)3·xH2O were added to a mixed solvent of 12 mL of oleic acid and 15 mL of 1-octadecene, and the mixture was heated at 130°C under vacuum for 30 min to form a lanthanum niobate complex and remove moisture; the solution was then cooled to 80°C in an argon atmosphere, and the β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticle dispersion was added to the solution, heated to 90°C, n-hexane was removed, and then the solution was cooled to 50°C, 10 mL of methanol solution containing NH4F (8 mmol) and NaOH (200 mg) was added, and stirred for 30 min, then methanol was removed, and then heated to 300°C under an argon atmosphere for 90 min; finally, cooled to room temperature, the solution was centrifuged to remove the solvent, and then washed with ethanol several times to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ Nanoparticles.

[0057] Figure 1 The transmission electron microscope images of the nanoparticles in each process of the preparation process of Example 1, where (a) and (b) are β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ Transmission electron microscope images of nanoparticles at different magnifications, (c) and (d) are β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Transmission electron microscope images of nanoparticles at different magnifications, (e) and (f) are β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticles transmission electron microscope images at different magnifications, (g) and (h) are β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er3+ Transmission electron microscope images of nanoparticles at different magnifications;

[0058] Figure 2 The nanoparticles prepared in Example 1 emit ultraviolet light under 980nm near-infrared light irradiation and emit blue-green light under 808nm irradiation. (d) and (e) are respectively the ultraviolet light emission under 980nm near-infrared light irradiation and the blue-green light emission under 808nm irradiation upconversion spectrum, (f) is the principle diagram of nanoparticle conversion spectrum. It can be seen from the figure that the synthesized β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ Nanoparticles can convert low-energy light into high-energy light, achieving orthogonal upconversion luminescence.

[0059] Figure 3 This is the XRD image of the nanoparticles prepared in Example 1. It can be seen from the figure that the prepared β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ The matrix of the nanoparticles is a β-NaYF4 crystal structure.

[0060] The various embodiments are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to in detail.

[0061] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A nanoparticle that emits ultraviolet and green light by orthogonal upconversion under near-infrared excitation, characterized in that: The chemical composition of the nanoparticles is: β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / He 3+ 。 2. The nanoparticles of claim 1 that emit ultraviolet and green light by near-infrared excitation orthogonal up-conversion, characterized in that: The nanoparticles are core-shell structures, specifically doped with an activator Tm 3+ and sensitizer Nd 3+ NaYF4 is used as the core, doped with Er 3+ and Yb 3+ NaF4 is the outer shell, and Nd is in the middle. 3+ The doped NaF4 is an optically inert layer and an inert isolation layer NaYF4.

3. The nanoparticles of claim 1 that emit ultraviolet and green light by near-infrared excitation orthogonal up-conversion, characterized in that: The β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ Medium Nd 3+ The molar concentration is 0.5-1mol%, Yb 3+ The molar concentration is 20-30 mol%, Tm 3+ The molar concentration is 0.5mol%; The β-NaYF4:Nd 3+ Medium Nd 3+ The molar concentration is 20-30 mol%; The NaYF4:Yb 3+ / Er 3+ Medium 3+ The molar concentration of Er is 18 mol%. 3+ The molar concentration is 2 mol%.

4. The nanoparticles of claim 1 that emit ultraviolet and green light by near-infrared excitation orthogonal up-conversion, characterized in that: The nanoparticles emit ultraviolet light when near-infrared light with a wavelength of 980 nm is used as an excitation source, and emit an up-conversion spectrum of blue-green light when near-infrared light with a wavelength of 808 nm is used as an excitation source.

5. The nanoparticles of claim 1 that emit ultraviolet and green light by orthogonal upconversion of near-infrared excitation, characterized in that: The nanoparticles are prepared by thermal decomposition method.

6. A method for preparing near-infrared excited orthogonal up-conversion ultraviolet and green light emitting nanoparticles according to any one of claims 1 to 5, characterized in that: The specific steps include: (1) Y(CH3CO2)3·xH2O, Nd(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Tm(CH3CO2)3·xH2O were mixed and reacted at a constant temperature in a mixed solution of oleic acid and 1-octadecene after vacuum evacuation to form a complex. After cooling to room temperature, a methanol solution of NH4F and NaOH was added to react under an argon atmosphere. Finally, ethanol was added to precipitate the core β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ Nanoparticles were dispersed in n-hexane to obtain the core rare earth complex precursor; (2) Y(CH3CO2)3·xH2O and Nd(CH3CO2)3·xH2O are weighed, and after vacuuming in a mixed solution of oleic acid and 1-octadecene, the mixture is reacted at a constant temperature to form a complex, and then the nuclear rare earth complex precursor obtained in step (1) is added, and the n-hexane is removed by heating. After cooling to room temperature, a methanol solution of NH4F and NaOH is added, and the mixture is reacted under an argon environment to obtain β-NaYF4:Nd 3+ / Yb 3 + / Tm 3+ @β-NaYF4:Nd 3+ Nanoparticles were dispersed in n-hexane to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ Nanoparticle dispersion; (3) Y(CH3CO2)3·xH2O is weighed and subjected to constant temperature reaction in a mixed solution of oleic acid and 1-octadecene after vacuuming to form a complex, and then the β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ The nanoparticle dispersion was heated to remove n-hexane, and after cooling to room temperature, NH4F and NaOH methanol solution were added to react under argon environment to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticles are dispersed in n-hexane to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4 nanoparticle dispersion; (4) Y(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Er(CH3CO2)3·xH2O are weighed, and a mixed solution of oleic acid and 1-octadecene is evacuated and reacted at a constant temperature to form a complex, and then the nanoparticle dispersion obtained in step (2) is added and heated to remove n-hexane. After cooling to room temperature, a methanol solution of NH4F and NaOH is added and reacted under an argon environment to obtain β-NaYF4:Nd 3+ / Yb 3+ / Tm 3+ @β-NaYF4:Nd 3+ @β-NaYF4@NaYF4:Yb 3+ / Er 3+ Nanoparticles.

7. The method for preparing nanoparticles emitting ultraviolet and green light by near-infrared excitation orthogonal up-conversion according to claim 6, characterized in that: The mass ratio of Y(CH3CO2)3·xH2O, Nd(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Tm(CH3CO2)3·xH2O in step (1) is 380-400:6-7:25-26:4-5; The mass ratio of Y(CH3CO2)3·xH2O to Nd(CH3CO2)3·xH2O in step (2) is 380-420:72-75; The mass ratio of Y(CH3CO2)3·xH2O, Yb(CH3CO2)3·xH2O and Er(CH3CO2)3·xH2O in step (4) is 380-420:102-105:13-14; The mass ratio of Y(CH3CO2)3·xH2O in steps (1), (2), (3) and (4) is 1:1:1:

1.

8. The method for preparing nanoparticles that emit ultraviolet and green light by near-infrared excitation orthogonal up-conversion according to claim 6, characterized in that: The isothermal reaction conditions in steps (1), (2), (3) and (4) are: reaction at 130° C. for 30-60 min; The reaction under argon environment in steps (1), (2), (3) and (4) is as follows: after removing methanol, react at 300° C. for 60-90 minutes.

9. Application of the near-infrared excited orthogonal up-conversion nanoparticles emitting ultraviolet and green light according to any one of claims 1 to 5 or the near-infrared excited orthogonal up-conversion nanoparticles emitting ultraviolet and green light obtained by the preparation method according to any one of claims 6 to 9 in optical imaging technology and biomedicine.