Magnetic nano fluorescence sensor based on rhodamine derivative, preparation method and application of magnetic nano fluorescence sensor in Co ion detection

By coupling rhodamine-PEG-N-hydroxysuccinimide to the surface of magnetic Fe3O4 nanoparticles, a magnetic nanofluorescence sensor was prepared, which solved the complexity of cobalt ion detection method and secondary pollution, and achieved rapid cobalt ions , simple and efficient detection, and high selectivity and sensitivity.

CN118909616APending Publication Date: 2024-11-08JIANGSU UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410974298.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing cobalt ion detection methods are complex in operation, require expensive instruments, and have secondary pollution problems. The preparation process of cobalt ion fluorescent probes is complicated and difficult to recover and utilize, and the detection effect is poor.

Method used

By coupling rhodamine-PEG-N-hydroxysuccinimide to the surface of magnetic Fe3O4 nanoparticles, a magnetic nanofluorescence sensor was prepared, and its magnetism was used to quickly separate under the external magnetic field to achieve rapid detection of cobalt ions and avoid secondary contamination. .

Benefits of technology

It realizes fast, simple and efficient detection of cobalt ions, with high selectivity and sensitivity, and avoids secondary pollution through magnetic separation, simplifying the detection process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909616A_ABST
    Figure CN118909616A_ABST
Patent Text Reader

Abstract

The invention discloses a magnetic nano fluorescence sensor based on a rhodamine derivative, a preparation method of the magnetic nano fluorescence sensor and application of the magnetic nano fluorescence sensor to detection of Co ions. The magnetic nano fluorescence sensor comprises aminated Fe3O4 nanoparticles and rhodamine-PEG-N-hydroxysuccinimide, and the rhodamine-PEG-N-hydroxysuccinimide is grafted on the surface of the Fe3O4 nano particle through a-CO-NH-bond. Rhodamine-PEG-N-hydroxysuccinimide (RB-PEG-NHS) fluorescent molecules are coupled to the surfaces of magnetic Fe3O4 nanoparticles, the magnetic nano fluorescence sensor can realize rapid detection of Co < 2 + > in wastewater, the selectivity is high, the sensitivity is high, the detected sensor can be rapidly enriched and separated from a water body under the action of an external magnetic field by utilizing the magnetism of the sensor, and the detection result is accurate. And secondary pollution is effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a magnetic nano fluorescence sensor based on rhodamine derivatives, a preparation method and application thereof in detecting Co ions, and belongs to the technical field of new material preparation and metal ion sensing detection in water bodies. Background Art

[0002] Heavy metal cobalt ions (Co 2+ ) concentration exceeding the standard will cause many pollution problems, such as low blood pressure, paralysis, diarrhea, etc., and will also cause gene mutations in living cells. 2+ When the concentration reaches 10mg / L, crucian carp and silk fish will die, causing great harm to the ecosystem and human health. Therefore, the identification and detection of cobalt ions are of great significance in the fields of environmental science, medicine and life science.

[0003] There are many methods for detecting cobalt ions that have been publicly reported, such as spectrophotometry, inductively coupled plasma mass spectrometry and atomic absorption spectrometry, but these methods are usually complicated to operate and require the use of expensive detection instruments. Their promotion and application are greatly limited. Therefore, it is of great significance to develop new cobalt ion detection methods.

[0004] Cobalt ion fluorescent probes have attracted much attention due to their advantages such as simple operation, no need for expensive instruments, good detection effect, and high sensitivity, such as Chinese patents CN117805040A, CN102735663A, and CN115028578A. Although these reported probes have high sensitivity and selectivity, they still have many problems such as complex preparation process, high detection limit, and poor practical application effect. In addition, these probes are difficult to recycle, and auxiliary separation is required repeatedly during preparation and use, and a large number of probes need to be invested in the detection process, which is easy to cause secondary pollution. Summary of the invention

[0005] The purpose of the present invention is to provide a magnetic nanofluorescence sensor based on rhodamine derivatives, a preparation method and its application in detecting Co ions, by coupling rhodamine-PEG-N-hydroxysuccinimide (RB-PEG-NHS) fluorescent molecules to the surface of magnetic Fe3O4 nanoparticles, which can realize the detection of Co in wastewater. 2+ It has rapid detection, strong selectivity and high sensitivity. After detection, the sensor can use its own magnetism to quickly enrich and separate from the water body under the action of an external magnetic field, effectively avoiding secondary pollution.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A magnetic nano fluorescence sensor based on rhodamine derivatives comprises amino-modified Fe3O4 nanoparticles and rhodamine-PEG-N-hydroxysuccinimide, wherein the rhodamine-PEG-N-hydroxysuccinimide is grafted onto the surface of the Fe3O4 nanoparticles via a -CO-NH- bond.

[0008] The preparation method of the magnetic nano-fluorescence sensor based on rhodamine derivatives comprises the following steps:

[0009] S1. Dispersing 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and N-hydroxysuccinimide in a buffer solution, adding Fe3O4-PAA nanoparticles, and stirring to activate; then adding 1,6-hexanediamine and triethanolamine in a stirring state to react, separating and washing after the reaction to obtain Fe3O4-NH2 nanoparticles, i.e., amination Fe3O4 nanoparticles;

[0010] S2. Disperse Fe3O4-NH2 nanoparticles in a buffer solution, add 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and rhodamine-PEG-N-hydroxysuccinimide, and separate, wash and dry after the reaction in the dark to obtain a magnetic nanofluorescence sensor.

[0011] Preferably, in step S1, the concentrations of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide in the buffer solution are both 15-30 mg / mL;

[0012] The mass ratio of Fe3O4-PAA nanoparticles, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide is (0.5-1.5):(2.3-3.5):(2.3-3.5).

[0013] Preferably, in step S1, the mass ratio of 1,6-hexanediamine, triethanolamine and Fe3O4-PAA nanoparticles is (0.2-0.6):(0.3-0.7):(0.03-0.1).

[0014] Preferably, the stirring activation conditions are: 3-8h at room temperature;

[0015] After adding 1,6-hexanediamine, the stirring reaction time is 20-35h;

[0016] After adding triethanolamine, the stirring reaction time is 0.2-1h.

[0017] Preferably, in step S1, the preparation method of Fe3O4-PAA nanoparticles is:

[0018] Polyacrylic acid, FeCl3·6H2O and anhydrous sodium acetate are dissolved in ethylene glycol in a mass ratio of 1:(1-3):(10-15), reacted at 180-250°C for 8-12h, separated and washed, and then dried at 30-50°C under vacuum conditions to obtain Fe3O4-PAA nanoparticles.

[0019] Preferably, in step S2, the mass ratio of Fe3O4-NH2 nanoparticles, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and rhodamine-PEG-N-hydroxysuccinimide is (0.4-0.7):(0.3-0.5):(0.02-0.1).

[0020] The above-mentioned magnetic nanofluorescence sensor based on rhodamine derivatives or the magnetic nanofluorescence sensor based on rhodamine derivatives prepared by any of the above-mentioned methods is used in detecting Co ions, specifically, adding the magnetic nanofluorescence sensor sub-sensor into wastewater and oscillating it, and reflecting the Co ions in the wastewater through fluorescence monitoring of the wastewater. 2+ The presence or absence of ions and Co 2+ Ion content.

[0021] A method for determining whether Fe3O4-PAA nanoparticles are aminated is provided, wherein 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide are dispersed in a buffer solution, and then Fe3O4-PAA nanoparticles are added and stirred for activation; then, 1,6-hexanediamine and triethanolamine are added in succession under stirring to react, and after the reaction is completed, the product is separated and washed to obtain the product, and the saturation magnetization value of the product is used as a basis for determining whether Fe3O4-PAA nanoparticles are aminated;

[0022] The saturation magnetization value of the product is lower than that of Fe3O4-PAA nanoparticles, indicating that the Fe3O4-PAA nanoparticles are amino-ated.

[0023] A method for determining whether rhodamine-PEG-N-hydroxysuccinimide is grafted on the surface of aminated Fe3O4-PAA nanoparticles is provided, which comprises dispersing 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and N-hydroxysuccinimide in a buffer solution, adding Fe3O4-PAA nanoparticles, and stirring for activation; then, adding 1,6-hexanediamine and triethanolamine in a stirring state to react, and obtaining Fe3O4-NH2 nanoparticles after separation and washing after the reaction is completed;

[0024] The Fe3O4-NH2 nanoparticles are then dispersed in a buffer solution, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and rhodamine-PEG-N-hydroxysuccinimide are added, and the reaction is carried out in the dark. After separation, washing and drying to obtain the product, the saturation magnetization intensity value of the product is used as a basis for judging whether rhodamine-PEG-N-hydroxysuccinimide is grafted onto the surface of the amino-Fe3O4-PAA nanoparticles;

[0025] The saturation magnetization value of the product was lower than that of Fe3O4-NH2 nanoparticles, indicating that rhodamine-PEG-N-hydroxysuccinimide was grafted onto the surface of amino-Fe3O4-PAA nanoparticles.

[0026] The beneficial effects of the present invention are:

[0027] The magnetic nanofluorescence sensor was prepared by coupling RB-PEG-NHS fluorescent molecules to the surface of Fe3O4-NH2 magnetic nanoparticles. 2+ It exhibits excellent recognition ability and can perform rapid qualitative and quantitative analysis of cobalt ions in solution; and the presence of magnetic nanoparticles enables the sensor to be separated from the solution quickly, simply and efficiently without causing secondary contamination. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 TEM images of Fe3O4-PAA and Fe3O4@PEG-RB prepared in Example 3;

[0029] Figure 2 VSM images of Fe3O4-PAA, Fe3O4-NH2 and Fe3O4@PEG-RB prepared in Example 3, and the inset is the physical image of the magnetic response of Fe3O4@PEG-RB;

[0030] Figure 3 XRD patterns of Fe3O4-PAA, Fe3O4-NH2 and Fe3O4@PEG-RB prepared in Example 3;

[0031] Figure 4 FT-IR images of Fe3O4-PAA, Fe3O4-NH2 and Fe3O4@PEG-RB prepared in Example 3;

[0032] Figure 5 The stability of the Fe3O4@PEG-RB magnetic nanosensor prepared in Example 3 under different pH environments;

[0033] Figure 6The specificity results of the Fe3O4@PEG-RB sensor prepared in Example 3, where (a) is the fluorescence spectrum of Fe3O4@PEG-RB when it coexists with different ions at 576nm, and (b) is the fluorescence spectrum of Fe3O4@PEG-RB to Co when competing ions coexist. 2+ Selectivity;

[0034] Figure 7 The sensitivity results of the Fe3O4@PEG-RB sensor prepared in Example 3, where (a) is the fluorescence intensity at 576 nm as Co 2+ (b) shows the change of sensor response rate and Co 2+ The relationship between concentration. DETAILED DESCRIPTION

[0035] The present invention will be specifically described below in conjunction with the accompanying drawings and embodiments.

[0036] Example 1

[0037] This embodiment provides an environmentally friendly, renewable Fe3O4 magnetic nanoparticle-based method for detecting Co 2 + The ion sensor Fe3O4@PEG-RB, the specific preparation method includes the following steps:

[0038] 0.151 g PAA (polyacrylic acid) was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC (anhydrous sodium acetate) were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0039] 75mg of Fe3O4-PAA was prepared, 200mg of EDC (1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride) and 200mg of NHS (N-hydroxysuccinimide) were dispersed in 10mL of PBS (phosphate buffer), and activated at room temperature for 4h. Then, 0.5mL of 7.66mol / L 1,6-hexanediamine was added, and the reaction was continued with stirring for 24h. Then, 0.5mL of 7.54mol / L triethanolamine was added, and the reaction was continued with stirring for 0.5h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained after magnetic separation and washing with deionized water 3 times.

[0040] 75 mg of Fe3O4-NH2 nanoparticles prepared above were dispersed in 10 mL PBS, and 50 mg of EDC and 10 mg of RB-PEG-NHS (rhodamine-PEG-N-hydroxysuccinimide, purchased from Aladdin) were added, and the reaction was carried out at room temperature in the dark for 24 h. After the reaction was completed, the Fe3O4@PEG-RB sensor was obtained by magnetic separation, washing with deionized water twice, and vacuum drying at 30 °C.

[0041] Example 2

[0042] 0.052 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol for three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0043] 75 mg Fe3O4-PAA was prepared, 200 mg EDC and 200 mg NHS were dispersed in 10 mL PBS, and activated at room temperature for 4 h. Then 0.5 mL 7.66 mol / L 1,6-hexanediamine was added, and the reaction was continued for 24 h. Then 0.5 mL 7.54 mol / L triethanolamine was added, and the reaction was continued for 0.5 h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained after magnetic separation and washing with deionized water for 3 times.

[0044] 75 mg of Fe3O4-NH2 nanoparticles prepared above were dispersed in 10 mL of PBS, and 50 mg of EDC and 5 mg of RB-PEG-NHS were added, and the mixture was reacted at room temperature in the dark for 24 h. After the reaction was completed, the Fe3O4@PEG-RB sensor was obtained by magnetic separation, washing with deionized water twice, and vacuum drying at 30 °C.

[0045] Example 3

[0046] 0.248 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol for three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0047] 75 mg of Fe3O4-PAA, 200 mg of EDC and 200 mg of NHS were dispersed in 10 mL of PBS and activated at room temperature for 4 h. Then, 0.5 mL of 7.66 mol / L 1,6-hexanediamine was added and the reaction was continued for 24 h. Then, 0.5 mL of 7.54 mol / L triethanolamine was added and the reaction was continued for 0.5 h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained after magnetic separation and washing with deionized water for 3 times.

[0048] 75 mg of Fe3O4-NH2 nanoparticles prepared above were dispersed in 10 mL PBS, and 50 mg of EDC and 10 mg of RB-PEG-NHS were added, and the mixture was reacted at room temperature in the dark for 24 h. After the reaction was completed, the Fe3O4@PEG-RB sensor was obtained by magnetic separation, washing with deionized water twice, and vacuum drying at 30 °C.

[0049] Example 4

[0050] 0.248 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol for three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0051] 75mg Fe3O4-PAA, 200mg EDC and 200mg NHS were dispersed in 10mL PBS and activated at room temperature for 4h. Then 0.5mL 7.66mol / L 1,6-hexanediamine was added and the reaction was continued for 24h. Then 0.7mL 7.54mol / L triethanolamine was added and the reaction was continued for 0.5h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained by magnetic separation and washing with deionized water for 3 times.

[0052] 75 mg of Fe3O4-NH2 nanoparticles prepared above were dispersed in 10 mL of PBS, and 50 mg of EDC and 8 mg of RB-PEG-NHS were added, and the mixture was reacted at room temperature in the dark for 24 h. After the reaction was completed, the Fe3O4@PEG-RB sensor was obtained by magnetic separation, washing with deionized water twice, and vacuum drying at 30 °C.

[0053] Example 5

[0054] 0.248 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol for three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0055] 75 mg of Fe3O4-PAA, 200 mg of EDC and 200 mg of NHS were dispersed in 10 mL of PBS and activated at room temperature for 4 h. Then, 0.7 mL of 7.66 mol / L 1,6-hexanediamine was added and the reaction was continued for 24 h. Then, 0.7 mL of 7.54 mol / L triethanolamine was added and the reaction was continued for 0.5 h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained after magnetic separation and washing with deionized water for 3 times.

[0056] 75 mg of Fe3O4-NH2 nanoparticles prepared above were dispersed in 10 mL PBS, and 50 mg of EDC and 12 mg of RB-PEG-NHS were added, and the mixture was reacted at room temperature in the dark for 24 h. After the reaction was completed, the Fe3O4@PEG-RB sensor was obtained by magnetic separation, washing with deionized water twice, and vacuum drying at 30 °C.

[0057] Example 6

[0058] 0.248 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol for three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0059] 75 mg of Fe3O4-PAA, 200 mg of EDC and 200 mg of NHS were dispersed in 10 mL of PBS and activated at room temperature for 4 h. Then, 0.7 mL of 7.66 mol / L 1,6-hexanediamine was added and the reaction was continued for 24 h. Then, 0.5 mL of 7.54 mol / L triethanolamine was added and the reaction was continued for 0.5 h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained after magnetic separation and washing with deionized water for 3 times.

[0060] 75 mg of Fe3O4-NH2 nanoparticles prepared above were dispersed in 10 mL of PBS, and 50 mg of EDC and 10 mg of RB-PEG-NHS were added, and the mixture was reacted at room temperature in the dark for 24 h. After the reaction was completed, the Fe3O4@PEG-RB sensor was obtained by magnetic separation, washing with deionized water twice, and vacuum drying at 30 °C.

[0061] Morphological characterization

[0062] The Fe3O4-PAA and Fe3O4@PEG-RB prepared in Example 3 were characterized by transmission electron microscopy (TEM). Figure 1 As shown in area a, the Fe3O4-PAA particles are spherical and evenly dispersed, with an average size of about 178 nm. Figure 1 The middle b area is the morphology of the prepared sensor Fe3O4@PEG-RB, which is also spherical in shape with an average diameter of about 223 nm, slightly larger than the particle size of Fe3O4-PAA. This is due to the amination of the Fe3O4-PAA surface and the grafting of the fluorescent molecule RB-PEG-NHS, which also confirms the successful preparation of the sensor Fe3O4@PEG-RB.

[0063] Magnetic properties test

[0064] The Fe3O4-PAA, Fe3O4-NH2 and Fe3O4@PEG-RB prepared in Example 3 were tested for magnetic properties by ADE EV7 vibrating sample magnetometer (VSM). Figure 2 As shown in the figure, it can be seen that the saturation magnetization value of Fe3O4-PAA (65.78emu / g) gradually decreases with surface modification (64.06emu / g) and RB-PEG-NHS coupling grafting (28.75emu / g). Because 1,6-hexanediamine, triethanolamine and RB-PEG-NHS are all non-magnetic, the saturation magnetization of Fe3O4-PAA is weakened, indicating that the amino group is successfully modified on the surface of Fe3O4-PAA and RB-PEG-NHS is effectively grafted onto Fe3O4-NH2. As shown in the attached figure Figure 2 As shown in the middle illustration, the prepared magnetic sensor Fe3O4@PEG-RB exhibits excellent magnetic properties, which enables the sensor to be quickly separated from the liquid in an external magnetic field environment to avoid secondary contamination.

[0065] Crystal form analysis

[0066] The Fe3O4-PAA, Fe3O4-NH2 and Fe3O4@PEG-RB sensors prepared in Example 3 were analyzed by X-ray powder diffractometer (XRD). Scanning range 20~70°. Figure 3 As shown, by comparing with the standard card (JCPDS no.19-629), it was found that the diffraction peaks of 2θ at 30.23°, 35.37°, 43.29°, 56.72°, and 63.14° are consistent with the (220), (311), (400), (511), and (440) crystal planes of Fe3O4, indicating that the modification and grafting process does not affect the crystal form of Fe3O4, and the prepared sensor has a good crystal structure.

[0067] Surface structure analysis

[0068] The Fe3O4-PAA, Fe3O4-NH2 and Fe3O4@PEG-RB sensors prepared in Example 3 were analyzed for their surface structures using an IR200 Fourier transform infrared spectrometer (FT-IR). An appropriate amount of the sample to be tested was prepared using the KBr tablet method with a scanning range of 4000 cm -1 ~500cm -1 . As attached Figure 4 As shown, 587cm -1 The absorption peak at is the typical Fe-O stretching vibration peak of Fe3O4. For Fe3O4-PAA nanoparticles ( Figure 4 Middle a area), 3465cm -1 The broad absorption peak at 1553 cm is caused by the stretching vibration of -OH of PAA. -1 and 1413cm -1 The peaks at are related to the stretching vibrations of C=O and CO, respectively, and the results show that Fe3O4-PAA was successfully prepared. Figure 4 As shown in area b, after amination, the characteristic peaks of C=O and CO disappear, and 3415 cm -1 The signal appearing at 1635 cm is the stretching vibration of NH. -1 The characteristic peak at 885 cm is attributed to the characteristic peak of the amide bond formed between PAA and primary amine. -1 The peak at corresponds to the rocking vibration of CN, which is consistent with the absorption peak of 1,6-hexanediamine, all of which indicate that Fe3O4-NH2 was successfully prepared through amide condensation reaction. The infrared absorption peak of Fe3O4@PEG-RB is shown in Figure 4 As shown in the middle c area, 3355cm -1 This corresponds to the strong absorption peak of -OH in PEG, 1655 cm -1 The peak at 1763 cm is attributed to the characteristic peak of the amide bond formed between the fluorescent molecule with activated NHS ester and the primary amine. -1 The peak at 1568 cm is attributed to the C=O stretching vibration of the ester in RB-PEG-NHS. -1 、1473cm -1and 1409cm -1 The peak at corresponds to the skeleton vibration of the benzene ring in RB-PEG-NHS, further confirming the successful preparation of the sensor Fe3O4@PEG-RB.

[0069] Application Example 1

[0070] The Fe3O4@PEG-RB sensor prepared in Example 3 was used to perform a divalent cobalt ion sensing test, which includes the following steps:

[0071] Weigh a certain amount of Fe3O4@PEG-RB sensor and disperse it in a certain volume of ultrapure water by ultrasonic to prepare the sensor stock solution (concentration is 1 mg / mL). Weigh appropriate amounts of FeCl3·6H2O, KCl, NH4Cl, CaCl2, NaCl, MnCl2, SnCl2·2H2O, CoCl2·6H2O, ZnCl2, CdCl2·2.5H2O and CuSO4·5H2O and dissolve them in ultrapure water to prepare a competitive ion stock solution with a concentration of 100 μmol / L. Dilute the pre-prepared CoCl2·6H2O mother solution with a concentration of 500 μmol / L to prepare a 100 μmol / LCoCl2·6H2O stock solution.

[0072] First, the stability of Fe3O4@PEG-RB in different pH environments (pH 1-14) was studied. Then, the sensor stock solution was mixed with the competitive ion stock solution according to the concentration and ratio designed in the experiment. After ultrasonic vibration for 30 seconds, it was allowed to stand for 15 minutes, and then the fluorescence spectrum test was performed. 2+ The obtained spectra were analyzed and studied to evaluate the sensor's performance on Co 2+ Next, Co 2+ After the mother solution is diluted in proportion (0.1-300 μmol / L), the same volume of sensor stock solution is added to the same volume of Co 2+ The solution was ultrasonically shaken for 30 seconds and then left to stand for 10 minutes to test the fluorescence intensity and analyze the sensor's response to Co 2+ response sensitivity.

[0073] As attached Figure 5As shown in the figure, the study of different acid-base environments shows that the fluorescence intensity of the Fe3O4@PEG-RB magnetic nanosensor has three mutations in the pH range of 1-14, namely 4, 11 and 14, and the fluorescence intensity under other pH conditions is almost unchanged. When the environmental pH value is 4, the measured solution fluorescence intensity is the largest. Therefore, in the experiment, the solution pH is controlled at about 4 as much as possible to obtain the best test effect. The same amount of the magnetic nanosensor suspension prepared in Example 3 was added to the same amount of 11 metal ion solutions of the same concentration, and the fluorescence intensity was tested after ultrasonic vibration for 30 seconds and then allowed to stand for 10 minutes. The results are shown in the attached figure. Figure 6 As shown in area a. Figure 6 It can be seen that Na + , K + NH4 + , Mn 2+ 、Zn 2+ , Ca 2+ Sn 2+ 、Cd 2+ , Cu 2+ , Fe 3+ There was no obvious fluorescence signal change in the metal ion solution, while Co 2+ The strong fluorescence intensity at 576 nm further confirmed that the magnetic nanosensor can specifically recognize Co 2+ , and the complex product has a strong fluorescence signal. Figure 6 As shown in area b, under the same conditions, Co 2+ The fluorescence intensity of the competitive ion solution containing the sensor was significantly enhanced, which means that the coexistence of various competitive ions will not affect the Fe3O4@PEG-RB to Co 2+ This indicates that the Fe3O4@PEG-RB sensor prepared in the present invention has high specificity.

[0074] In addition, with the 2+ With the increase of concentration, the fluorescence intensity at 576nm gradually increased (see Figure 7 The F / F0 value and Co 2+ The change of fluorescence spectrum was evaluated as a function of concentration. In the concentration range of 0.1 to 60 μM, the F / F0 value was significantly related to Co 2+ The concentration has a good linear relationship ( Figure 7 b area), y = 0.0858x + 1.2974, (R 2 =0.9922), according to the detection limit LOD = 3s b / S, where sb and S are the standard deviation of the blank sample and the slope of the linear fitting equation, respectively. The LOD value of the sensor prepared in Example 3 was calculated to be 0.083 μM, which is less than the limit of cobalt content in drinking water stipulated by my country (1.7 μM 3838-2002 "Surface Water Environmental Quality Standard"). It can be seen that the Fe3O4@PEG-RB sensor has good sensitivity. 2+ It has shown great application potential in the field of wastewater detection and deep treatment.

[0075] The Fe3O4@PEG-RB sensor prepared in other embodiments of the present invention also has excellent performance similar to that of the sensor prepared in Example 3, with high sensitivity, strong specificity and easy recovery.

[0076] Comparative Example 1

[0077] 0.248 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol for three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0078] The product of Comparative Example 1 was subjected to Co 2+ The ion sensing test found that there was no obvious fluorescence change before and after sensing, and it did not have the sensing detection function.

[0079] Comparative Example 2

[0080] 0.248 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 200 °C for 10 h. After cooling to room temperature, it was magnetically separated, washed with deionized water and ethanol for three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles.

[0081] 75 mg of Fe3O4-PAA, 200 mg of EDC and 200 mg of NHS were dispersed in 10 mL of PBS and activated at room temperature for 4 h. Then, 0.5 mL of 7.66 mol / L 1,6-hexanediamine was added and the reaction was continued for 24 h. Then, 0.5 mL of 7.54 mol / L triethanolamine was added and the reaction was continued for 0.5 h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained after magnetic separation and washing with deionized water for 3 times.

[0082] The sensing performance study found that the product Fe3O4-NH2 obtained in Comparative Example 2 did not have obvious fluorescence changes before and after sensing under the same detection conditions compared to the sensor Fe3O4@PEG-RB prepared in Example 3, and did not have the sensing detection function.

[0083] Comparative Example 3

[0084] 0.248 g PAA was weighed and dissolved in 40 mL ethylene glycol, stirred in a 50 °C water bath until completely dissolved, then 0.5 g FeCl3·6H2O and 3.0 g NaAC were added, and after ultrasonic dissolution, the mixture was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, reacted at 200 °C for 10 h, cooled to room temperature, separated by magnetic separation, washed with deionized water and ethanol three times respectively, and dried in vacuo at 35 °C to obtain Fe3O4-PAA nanoparticles;

[0085] 75mg Fe3O4-PAA, 200mg EDC and 200mg NHS were dispersed in 10mL PBS, stirred and activated at room temperature for 4h, then 0.5mL 7.66mol / L 1,6-hexanediamine was added, and the reaction was continued with stirring for 24h. Then 0.7mL 7.54mol / L triethanolamine was added, and the reaction was continued with stirring for 0.5h. After the reaction was completed, the Fe3O4-NH2 nanoparticles were obtained after magnetic separation and washing with deionized water 3 times.

[0086] 75 mg of Fe3O4-NH2 nanoparticles prepared above were dispersed in 10 mL of PBS, and 50 mg of EDC and 5 mg of RB-PEG-NHS were added, and the mixture was reacted at room temperature in the dark for 24 h. After the reaction was completed, the Fe3O4@PEG-RB sensor was obtained by magnetic separation, washing with deionized water twice, and vacuum drying at 30 °C.

[0087] The sensing performance study found that under the same detection environment, the sensor prepared in Comparative Example 3 had a longer sensing time (16 minutes of standing after 1 minute of shaking) than the sensor prepared in Example 3. 2+ The sensitivity is poor in an environment with a higher concentration (>100 μM), which is due to the fact that the amount of RB-PEG-NHS added in Comparative Example 3 is small, resulting in a lower effective grafting rate.

[0088] The above is only a preferred implementation of the patent of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the patent of the present invention. These improvements and modifications should also be regarded as the scope of protection of the patent of the present invention.

Claims

1. A magnetic nanofluorescence sensor based on rhodamine derivatives, It is characterized in that Including amino Fe 3 O 4 Nanoparticles and rhodamine-PEG-N-hydroxysuccinimide, and rhodamine-PEG-N-hydroxysuccinimide is grafted to Fe via a -CO-NH- bond 3 O 4 Nanoparticle surface.

2. The method for preparing the magnetic nano-fluorescence sensor based on rhodamine derivatives according to claim 1, It is characterized in that The steps include: S1. Disperse 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and N-hydroxysuccinimide in a buffer solution, and then add Fe 3 O 4 -PAA nanoparticles, stirring to activate; then adding 1,6-hexanediamine and triethanolamine successively under stirring to react, after the reaction is completed, separating and washing to obtain Fe 3 O 4 -NH 2 Nanoparticles, namely, amination of Fe 3 O 4 Nanoparticles; S2, Fe 3 O 4 -NH 2 The nanoparticles are dispersed in a buffer solution, and then 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and rhodamine-PEG-N-hydroxysuccinimide are added. After the reaction is protected from light, the magnetic nanofluorescence sensor is obtained by separation, washing and drying.

3. The method for preparing the magnetic nano-fluorescence sensor based on rhodamine derivatives according to claim 2, It is characterized in that In step S1, the concentrations of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide in the buffer solution are both 15-30 mg / ml; Fe 3 O 4 The mass ratio of -PAA nanoparticles, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide is (0.5-1.5):(2.3-3.5):(2.3-3.5).

4. The method for preparing the magnetic nano-fluorescence sensor based on rhodamine derivatives according to claim 2, It is characterized in that In step S1, 1,6-hexanediamine, triethanolamine and Fe 3 O 4 -The mass ratio of PAA nanoparticles is (0.2-0.6):(0.3-0.7):(0.03-0.1).

5. The method for preparing the magnetic nano-fluorescence sensor based on rhodamine derivatives according to claim 2, It is characterized in that The conditions for stirring activation are: 3-8h at room temperature; After adding 1,6-hexanediamine, the stirring reaction time is 20-35h; After adding triethanolamine, the stirring reaction time is 0.2-1h.

6. The method for preparing the magnetic nano-fluorescence sensor based on rhodamine derivatives according to claim 2, It is characterized in that In step S1, Fe 3 O 4 -PAA nanoparticles are prepared by: Polyacrylic acid, FeCl 3 6H 2 O and anhydrous sodium acetate are dissolved in ethylene glycol in a mass ratio of 1:(1-3):(10-15), reacted at 180-250°C for 8-12h, separated and washed, and then dried at 30-50°C under vacuum to obtain Fe 3 O 4 -PAA nanoparticles.

7. The method for preparing the magnetic nano-fluorescence sensor based on rhodamine derivatives according to claim 2, It is characterized in that In step S2, Fe 3 O 4 -NH 2 The mass ratio of nanoparticles, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and rhodamine-PEG-N-hydroxysuccinimide is (0.4-0.7):(0.3-0.5):(0.02-0.1).

8. Use of the magnetic nanofluorescence sensor based on rhodamine derivatives according to claim 1 or the magnetic nanofluorescence sensor based on rhodamine derivatives prepared by the method described in any one of claims 2 to 7 in detecting Co ions.

9. A kind of Fe 3 O 4 -Method for determining the amination of PAA nanoparticles, It is characterized in that The method is to disperse 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and N-hydroxysuccinimide in a buffer solution and then add Fe 3 O 4 -PAA nanoparticles, stirred and activated; then, under stirring, 1,6-hexanediamine and triethanolamine were added successively to react. After the reaction was completed, the product was separated and washed to obtain the product. The saturation magnetization intensity value of the product was used as the judgment of Fe 3 O 4 -Basis for the amination of PAA nanoparticles; The saturation magnetization of the product is lower than that of Fe 3 O 4 The saturation magnetization value of -PAA nanoparticles indicates that Fe 3 O 4 -PAA nanoparticles are amino-ated.

10. Ammoniated Fe 3 O 4 - Determination method of rhodamine-PEG-N-hydroxysuccinimide grafted on the surface of PAA nanoparticles, It is characterized in that The method is to disperse 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and N-hydroxysuccinimide in a buffer solution and then add Fe 3 O 4 -PAA nanoparticles, stirred and activated; then, under stirring, 1,6-hexanediamine and triethanolamine were added successively to react, and after the reaction was completed, Fe 3 O 4 -NH 2 Nanoparticles; Then Fe 3 O 4 -NH 2 The nanoparticles were dispersed in a buffer solution, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and rhodamine-PEG-N-hydroxysuccinimide were added, and the reaction was carried out in the dark. After separation, washing and drying, the product was obtained. The saturation magnetization intensity value of the product was used as a judgement to determine whether rhodamine-PEG-N-hydroxysuccinimide was grafted onto the amino-Fe 3 O 4 -Basis for grafting PAA nanoparticle surface; The saturation magnetization of the product is lower than that of Fe 3 O 4 -NH 2 The saturation magnetization value of the nanoparticles indicates that rhodamine-PEG-N-hydroxysuccinimide is grafted onto the amino-Fe 3 O 4 -PAA nanoparticle surface.

Citation Information

Cited By

  • Cyclodextrin bionic organic iridium magnetic catalyst as well as preparation method and application thereof

    CN119303635A