Phase shift mask corrosive liquid as well as preparation method and application thereof
By optimizing the composition of the phase shift mask corrosion liquid, including silicon-based, chromium-based and molybdenum silicon-based film corrosion liquid, the problems of strict corrosion conditions, high cost and base layer corrosion in the existing technology are solved, and efficient and economical phase shift mask corrosion and rework effects.
Patent Information
- Application Number
- CN202410967462.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
When removing phase shift masks, the existing wet corrosion technology has strict corrosion conditions, high chemical raw materials prices, low corrosion rate, and it is difficult to avoid corrosion to the base layer, affecting the flatness and rework efficiency of the photomask.
Provide a phase shift mask corrosion liquid, including silicon-based film corrosion liquid, chromium-based film corrosion liquid and molybdenum-silicon film corrosion liquid, to improve the corrosion efficiency of the silicon-based film layer by optimizing the ratio of alkali and surfactant. , use acetic acid and ammonium hydrogen fluoride to replace traditional corrosion agents, reduce operational risks and costs, and ensure efficient corrosion of the chromium-based film layer and molybdenum-silicon film layer.
The corrosion rate and flatness of the phase shift mask are significantly improved, the corrosion conditions are broadened, the corrosion conditions are avoided, the production costs are reduced, and the efficient rework of the phase shift mask is achieved.
Smart Images

Figure CN118909632A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wet etching, and in particular to a phase-shift mask etching solution and a preparation method and application thereof. Background Art
[0002] Photomasks include binary masks, phase-shift masks, etc., among which the film structure of the phase-shift mask is relatively complex: it includes a molybdenum-containing silicon phase-shift film layer, a chromium-containing light-shielding layer, and a silicon-containing protective layer, which are stacked from the base layer (the material can be silicon dioxide). In the process of photomask production, it is inevitable that the photomask will be reworked due to defects caused by environmental or human factors. Conventional physical grinding to remove the film layer has defects such as incomplete removal, which may affect the flatness of the substrate.
[0003] In order to solve the above problems, some technologies have tried to remove the phase shift mask by wet etching. However, in the wet etching process, there are problems such as relatively harsh etching conditions, relatively expensive chemical raw materials, complex etching solution composition, and relatively low etching rate. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a phase shift mask etching solution, which can effectively improve the etching rate and etching flatness of the phase shift mask, broaden the optional etching conditions, and avoid corrosion of the substrate layer.
[0005] The invention also provides a method for preparing the phase-shift mask etching solution.
[0006] The invention also provides application of the phase-shift mask etching solution.
[0007] According to an embodiment of the first aspect of the present invention, a phase-shift mask etching solution is provided, wherein the phase-shift mask etching solution comprises a silicon-based film layer etching solution, a chromium-based film layer etching solution and a molybdenum-silicon film layer etching solution;
[0008] The raw materials for preparing the silicon-based film etching solution are as follows:
[0009] 300-600 parts of alkali;
[0010] 10-30 parts of surfactant;
[0011] 400 to 1000 parts of water.
[0012] The phase-shift mask etching solution according to the embodiment of the present invention has at least the following beneficial effects:
[0013] (1) The present invention provides a phase-shift mask etching solution, which includes a silicon-based film layer etching solution, a chromium-based film layer etching solution and a molybdenum-silicon film layer etching solution; thereby, the complete etching of the phase-shift mask can be achieved, the process is smoother, and the conditions for phase-shift mask etching are broadened.
[0014] (2) In the silicon-based film etching solution provided by the present invention, alkali is the main etchant of the silicon-based film layer, and its optimal concentration ratio can achieve the optimal etching selectivity of the silicon-based film layer (Si / SiO2). Specifically, the silicon in the silicon-based film layer can be removed first, and then the silicon dioxide in the base layer will be etched. In other words, by adjusting the alkali concentration, the corrosion of the base layer can be avoided. The surfactant plays an effective role in removing particles, and the appropriate amount can remove particles without leaving residues on the substrate.
[0015] On the whole, the phase-shift mask etching solution provided by the present invention can be used to rework the phase-shift mask more effectively, conveniently and practically.
[0016] According to some embodiments of the present invention, in the raw materials for preparing the silicon-based film layer etching solution, the alkali includes at least one of tetramethylammonium hydroxide (TMAH), sodium hydroxide (NaOH) and potassium hydroxide (KOH).
[0017] According to some embodiments of the present invention, in the raw materials for preparing the silicon-based film etching solution, the alkali is selected from potassium hydroxide. Compared with potassium hydroxide, the silicon-based film etching solution improves the etching efficiency of the silicon-based film layer by at least 10-20%. Compared with tetramethylammonium hydroxide, the effect of potassium hydroxide is equivalent or better, and the cost is significantly reduced.
[0018] According to some embodiments of the present invention, in the raw materials for preparing the silicon-based film etching solution, the surfactant includes at least one of an anionic surfactant and a non-ionic surfactant.
[0019] According to some embodiments of the present invention, in the raw materials for preparing the silicon-based film etching solution, the surfactant is selected from a non-ionic surfactant, so that no ion residue is generated, and a synergistic effect is produced between the surfactant and the potassium hydroxide, and the etching effect is improved by 10-20% compared with other alkali and surfactant combinations.
[0020] According to some embodiments of the present invention, the nonionic surfactant includes a fluorinated polyether surfactant, which has high surface activity, high thermodynamic and chemical stability, good ability to reduce interfacial tension, and better synergy with other preparation raw materials used in the present invention.
[0021] According to some embodiments of the present invention, the chemical formula of the nonionic surfactant is CF3O(CF2O): nCF2CONHCH2CH2CH2CH2N(CH3)2COONH4, wherein n=1 to 8. The nonionic surfactant is an oligomer, and the range of n indicates the degree of polymerization. On the one hand, a considerable technical effect can be achieved within this range; on the other hand, the oligomer is actually a mixture, and the mixture includes nonionic surfactants within the range of n=1 to 8.
[0022] According to some embodiments of the present invention, the raw materials for preparing the silicon-based film etching solution are, by weight:
[0023] 400-450 parts of alkali;
[0024] 15-20 parts of surfactant;
[0025] 800-850 parts of water.
[0026] For example, in the raw materials for preparing the silicon-based film etching solution, the mass ratio of the alkali to water is 50-55:100, for example, about 52:100 or about 53:100.
[0027] In the raw materials for preparing the silicon-based film etching solution, the mass ratio of the surfactant to water is 1.5 to 2.5:100, for example, about 1.8:100, 2:100 or about 2.3:100.
[0028] According to some embodiments of the present invention, the raw materials for preparing the chromium-based film etching solution include, by weight:
[0029] 100-200 parts of cerium nitrate ammonium;
[0030] 10-30 parts of acetic acid;
[0031] 200-800 parts of water.
[0032] In conventional technology, oxidizing acid and ammonium cerium nitrate are usually used together, but the operation of oxidizing acid is highly dangerous and may volatilize to produce harmful gases such as chlorine. The present invention creatively selects acetic acid and adjusts the concentration of ammonium cerium nitrate to achieve high stripping efficiency of the chromium-based film layer, significantly optimize the operating environment, and reduce production costs.
[0033] In the chromium-based film etching solution provided by the present invention, cerium nitrate ammonium plays a role in the corrosion of chromium, and the standard electrode potential of Ce(IV) / Ce(III) is about 1.61V, which is sufficient to oxidize Cr(III) to Cr(VI) (1.23V). If the concentration (dosage) is too high, it will easily lead to crystallization and poor dissolution, and if the concentration is too dilute, the chromium removal efficiency is low. Acetic acid can inhibit the hydrolysis of cerium nitrate ammonium and promote the corrosion of the chromium-based film layer.
[0034] According to some embodiments of the present invention, the raw materials for preparing the chromium-based film etching solution are, by weight:
[0035] 110-150 parts of cerium nitrate ammonium;
[0036] 12-18 parts of acetic acid;
[0037] 600-800 parts of water.
[0038] For example, in the raw materials for preparing the chromium-based film etching solution, the mass ratio of ammonium cerium nitrate to water is 14-18:100, for example, it can be about 15:100.
[0039] In the raw materials for preparing the chromium-based film etching solution, the mass ratio of acetic acid to water is 1.5 to 2:100, for example, specifically about 1.8:100.
[0040] According to some embodiments of the present invention, the raw materials for preparing the molybdenum-silicon film etching solution include, by weight:
[0041]
[0042] In the molybdenum-silicon film corrosion, the oxide oxidizes the molybdenum-silicon film to produce metal oxides, and the fluorine atoms in the ammonium bifluoride react with the metal ions in the metal oxide to form a water-soluble complex, which is easy to remove. The addition of sulfuric acid can make the etching rate of the molybdenum-silicon film greater than the etching rate of the substrate silicon dioxide, thereby avoiding the corrosion of the substrate silicon dioxide. That is, the amount of raw materials used can achieve the optimal economic cost and the etching selectivity ratio of the molybdenum-silicon film (MoSi / SiO2).
[0043] According to some embodiments of the present invention, in the raw materials for preparing the molybdenum-silicon film etching solution, the fluoride includes at least one of ammonium bifluoride and ammonium fluoride.
[0044] According to some embodiments of the present invention, in the raw materials for preparing the molybdenum-silicon film etching solution, the fluoride is selected from ammonium bifluoride. Therefore, per unit mass, the fluoride provides a higher concentration of fluoride ions, which can more effectively remove the silicon film layer.
[0045] According to some embodiments of the present invention, in the raw materials for preparing the molybdenum-silicon film etching solution, the oxidant includes at least one of hydrogen peroxide, periodic acid and sodium hypochlorite.
[0046] According to some embodiments of the present invention, the oxidant is selected from hydrogen peroxide. Thus, the cost of the phase-shift mask etching solution can be reduced on the basis of achieving equivalent or better technical effects.
[0047] According to some embodiments of the present invention, the raw materials for preparing the molybdenum-silicon film layer corrosion are, by weight:
[0048]
[0049] Specifically, in the raw materials for preparing the molybdenum-silicon film etching solution, the mass ratio of the fluoride to water is 2.5-3:100, for example, specifically about 2.8:100.
[0050] In the raw materials for preparing the molybdenum-silicon film etching solution, the mass ratio of sulfuric acid to water is 14-16:100, for example, specifically about 15:100.
[0051] In the raw materials for preparing the molybdenum-silicon film etching solution, the mass ratio of the oxidant to water is 20-25:100, for example, about 22:100, 23:100 or about 24:100.
[0052] According to an embodiment of the second aspect of the present invention, there is provided a method for preparing the phase-shift mask etching solution, comprising:
[0053] Mixing the raw materials for preparing the silicon-based film layer etching solution to obtain the silicon-based film layer etching solution;
[0054] Mixing the raw materials for preparing the chromium-based film layer etching solution to obtain the chromium-based film layer etching solution;
[0055] The raw materials for preparing the molybdenum-silicon film layer etching solution are mixed to obtain the molybdenum-silicon film layer etching solution.
[0056] Since the preparation method adopts all the technical solutions of the phase-shift mask etching solution of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0057] In the preparation method, the mixing method and mixing time of various preparation raw materials are not limited, and can be selected according to experimental conditions and other conditions in actual production, as long as uniform dispersion can be achieved.
[0058] According to an embodiment of the third aspect of the present invention, there is provided a method for removing a phase-shift mask using the phase-shift mask etching solution, wherein the phase-shift mask comprises a molybdenum-silicon film layer, a chromium-based film layer and a silicon-based film layer stacked and arranged starting from a silicon dioxide base layer; the method comprises the following steps:
[0059] S1. The phase shift mask is corroded in the silicon-based film layer etching solution; the etching temperature is 50 to 90°C;
[0060] S2. The component obtained in step S1 is corroded in the chromium-based film layer in the etching solution;
[0061] S3. Etching the component obtained in step S2 in the molybdenum-silicon film etching solution.
[0062] Since the method adopts all the technical solutions of the phase-shift mask etching solution of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0063] In the method provided by the present invention, by limiting the etching temperature in step S1, the etching of the silicon-based film layer can be achieved and significantly improved.
[0064] According to some embodiments of the present invention, the material of the silicon-based film layer includes silicon alone. Considering environmental influences such as storage, the silicon-based film layer also includes a small amount of silicon oxide.
[0065] According to some embodiments of the present invention, the thickness of the silicon-based film layer is 10-50 nm. This thin thickness shortens the time required for etching and removing, thereby reducing the corrosion damage of the silicon-based film layer etching solution to the silicon dioxide substrate layer.
[0066] According to some embodiments of the present invention, in step S1, the etching temperature is 60-80°C, for example, about 70°C.
[0067] According to some embodiments of the present invention, in step S1, the etching rate is 1-3 μm / min (for the silicon-based film layer)
[0068] According to some embodiments of the present invention, in step S1, the etching rate of the silicon-based film layer etching solution on the silicon dioxide base layer is 2-4 nm / min.
[0069] The etching temperature and the composition of the silicon-based film layer etching solution cause the above-mentioned difference in etching rate, thereby avoiding the influence of the etching in step S1 on the silicon dioxide base layer.
[0070] According to some embodiments of the present invention, in step S1, the duration of the corrosion is 0.2 to 4 seconds, for example, about 2 seconds or about 3 seconds.
[0071] According to some embodiments of the present invention, in step S1, the etching is performed under ultrasonic conditions. The frequency of the ultrasound used is 100 to 300 kHz. For example, it can be about 150 kHz, 200 kHz or about 250 kHz. Combined with the composition ratio of the silicon-based film layer etching solution, the etching rate of the silicon-based film layer can be significantly optimized, and no residue will be generated on the surface of the component after the etching is completed.
[0072] According to some embodiments of the present invention, in step S2, the etching temperature is 20-40°C, for example, about 25°C, 30°C or about 35°C.
[0073] According to some embodiments of the present invention, the chromium-based film layer comprises elemental chromium and chromium oxide.
[0074] According to some embodiments of the present invention, the thickness of the chromium-based film layer is 1-2 μm.
[0075] According to some embodiments of the present invention, in step S2, the corrosion rate is 0.2-0.4 μm / min.
[0076] According to some embodiments of the present invention, in step S2, the duration of the corrosion is 2.5 to 10 minutes, for example, specifically about 5 minutes.
[0077] Combined with the corrosion conditions in step S2 and the composition of the chromium-based film etching solution used, the optimal corrosion rate of the chromium-based film layer can be achieved. If the temperature and time are not within the above range, the corrosion time will be correspondingly extended, the volatility of the etching solution will be enhanced, and it will be unfavorable for operation. According to some embodiments of the present invention, in step S3, the corrosion temperature is 20 to 40°C. For example, it can be about 25°C, 30°C or about 35°C.
[0078] According to some embodiments of the present invention, the thickness of the molybdenum silicon film layer is 2-4 μm.
[0079] According to some embodiments of the present invention, in step S3, the etching rate is 5-10 nm / min.
[0080] According to some embodiments of the present invention, in step S3, the duration of the corrosion is 200 to 800 minutes, for example, about 300 minutes, 400 minutes or about 500 minutes.
[0081] The etching rate of the molybdenum-silicon film layer can be significantly optimized by combining the composition of the molybdenum-silicon film layer etching solution and the etching time in step S3.
[0082] According to some embodiments of the present invention, in the method, after each step is completed, the obtained component needs to be cleaned. This can avoid the corrosion liquid used in the previous step from contaminating the corrosion liquid in the subsequent step. The cleaning method includes spraying with clean water, and the spraying time is 3 to 8 minutes, for example, it can be about 5 minutes.
[0083] According to some embodiments of the present invention, the method further comprises subjecting the obtained component to water ultrasonic treatment after step S3, so as to further clean the obtained component and facilitate the reuse of the obtained component.
[0084] According to some embodiments of the present invention, the component obtained by the method is a crystallized silicon dioxide base layer (also called a quartz substrate). The quartz substrate is transparent and can be reused.
[0085] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.
[0086] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values 2 and 3.
[0087] Unless otherwise specified, the water used in the present invention has a purity ≥ deionized water, for example, it can be deionized water or ultrapure water.
[0088] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0089] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0090] Figure 1 This is a cross-sectional SEM of the phase-shift mask used in Example 2 of the present invention.
[0091] Figure 2 This is an apparent diagram of the phase-shift mask used in Example 2 of the present invention.
[0092] Figure 3 This is an apparent diagram of the component obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0093] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0094] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0095] Example 1
[0096] In this example, a phase shift mask etching solution is prepared, which is specifically composed of a silicon-based film layer etching solution, a chromium-based film layer etching solution and a molybdenum-silicon film layer etching solution; wherein:
[0097] By weight, the raw materials for preparing the silicon-based film etching solution are:
[0098] 400 parts of alkali (potassium hydroxide);
[0099] Surfactant (nonionic surfactant) 15 parts;
[0100] 800 parts of deionized water.
[0101] The nonionic surfactant in this example is model TD-1, and its structural formula is CF3O(CF2O) n CF2CONHCH2CH2CH2CH2N(CH3)2COONH4, wherein n=1~8.
[0102] By weight, the raw materials for preparing the chromium-based film etching solution are:
[0103] 120 parts of cerium nitrate ammonium;
[0104] Acetic acid (36wt%) 15 parts;
[0105] 800 parts of water.
[0106] By weight, the raw materials for preparing the molybdenum-silicon film etching solution are:
[0107]
[0108] The preparation method of the phase shift mask etching solution in this example is:
[0109] Mixing raw materials for preparing silicon-based film etching solution;
[0110] Mixing raw materials for preparing the chromium-based film etching solution;
[0111] The raw materials for preparing the molybdenum-silicon film etching solution are mixed.
[0112] The obtained silicon-based film layer etching solution, chromium-based film layer etching solution and molybdenum-silicon film layer etching solution are stored respectively.
[0113] Example 2
[0114] In this example, the phase-shift mask etching solution obtained in Example 1 is used to etch a phase-shift mask. Specifically:
[0115] refer to Figures 1-2 As shown, the phase-shift mask used in the present invention includes a molybdenum silicon film layer (3 μm), a chromium-based film layer (including chromium and chromium oxide, 1.5 μm thick) and a silicon-based film layer (including silicon and silicon oxide, 45 nm thick) stacked on a silicon dioxide base layer.
[0116] The specific steps of corrosion are:
[0117] S1. The phase-shift mask is ultrasonically corroded in a silicon-based film etching solution, the ultrasonic etching temperature is 70°C, the duration is 2s, and the ultrasonic frequency is 200kHz; after the ultrasonic etching is completed, the obtained component is sprayed with deionized water for 5 minutes.
[0118] S2. The component obtained in step S1 is corroded in a chromium-based film layer corrosive solution at a temperature of 30° C. for 5 minutes. After the corrosion is completed, the component is sprayed with deionized water for 5 minutes.
[0119] S3. The component obtained in step S2 is corroded in the molybdenum-silicon film layer corrosive solution; the corrosion temperature is 30° C., and the corrosion time is 300 min; after the corrosion is completed, the obtained component is sprayed with deionized water for 5 min.
[0120] S4. The components obtained in step S3 are ultrasonically cleaned with deionized water. The frequency of the ultrasound used is 200 kHz and the duration of the ultrasound is 5 minutes.
[0121] The appearance of the parts obtained in this example is as follows Figure 3 As shown; it can be seen from the appearance that in this example, the phase-shift mask can be completely removed through simple steps; and the surface of the obtained component (silicon dioxide base layer) is clean and flat, which shows that the phase-shift mask etching solution provided by the present invention hardly corrodes the silicon dioxide base layer, which can ensure the reuse of the obtained component.
[0122] Example 3
[0123] This example provides a phase shift mask etching solution, which is different from Example 1 in that:
[0124] By weight, the raw materials for preparing the silicon-based film etching solution are:
[0125] Alkali (potassium hydroxide) 450 parts;
[0126] Surfactant (nonionic surfactant) 20 parts;
[0127] 830 parts of deionized water.
[0128] The source and type of surfactant in this example are the same as those in Example 1.
[0129] Example 4
[0130] This example etches a phase shift mask, and the specific difference from Example 2 is that:
[0131] (1) The phase shift mask etching solution used is from Example 3.
[0132] The results show that the corrosion time of Example 4 is comparable to that of Example 2, which shows that adjusting the concentration of the silicon-based film etching solution within the range provided by the present invention has little effect on the corrosion rate. In addition, the corrosion time is very short, which can avoid damage to the silicon dioxide base layer in this step.
[0133] Example 5
[0134] This example provides a phase shift mask etching solution, which is different from Example 1 in that:
[0135] By weight, the raw materials for preparing the molybdenum-silicon film etching solution are:
[0136] Fluoride (ammonium bifluoride) 60 parts;
[0137] 300 parts of sulfuric acid;
[0138] Oxidant (hydrogen peroxide) 500 parts;
[0139] 2000 parts of deionized water.
[0140] The parameters of sulfuric acid and oxidant in this example are the same as those in Example 1.
[0141] Example 6
[0142] This example etches a phase shift mask, and the specific difference from Example 2 is that:
[0143] (1) The phase shift mask etching solution used is from Example 5.
[0144] (2) In step S3, the duration of the etching is 250 minutes. It can be seen that within the scope provided by the present invention, increasing the concentration of fluoride can accelerate the etching speed of the molybdenum-silicon film layer to a certain extent.
[0145] Example 7
[0146] This example provides a phase shift mask etching solution, which is different from Example 1 in that:
[0147] In the raw materials for preparing the silicon-based film etching solution, the surfactant is BASF Disponil FES 32 anionic surfactant.
[0148] Example 8
[0149] A phase shift mask is etched, which is different from Embodiment 2 in that:
[0150] (1) The phase shift mask etching solution used is from Example 7.
[0151] The results provided in this example show that the corrosion time of the silicon-based film layer is 4s, and there are impurities attached to the surface of the obtained component that are visible to the naked eye. This also shows that the synergy between the non-ionic surfactant and other ingredients is better.
[0152] Example 9
[0153] This example provides a phase shift mask etching solution, which is different from Example 1 in that:
[0154] Among the raw materials for preparing the molybdenum-silicon film etching solution, the oxidant is selected from periodic acid.
[0155] Example 10
[0156] A phase shift mask is etched, which is different from Embodiment 2 in that:
[0157] (1) The phase shift mask etching solution used is from Example 9.
[0158] The time required for etching the molybdenum-silicon film layer in this example is equivalent to that in Example 2, but there are impurities remaining on the surface of the component obtained by etching, and ultrasonic cleaning is required before the next step. It can be seen that when hydrogen peroxide is used as an oxidant, it has the advantage of low cost and can also avoid impurities.
[0159] Comparative Example 1
[0160] This example provides a phase shift mask etching solution, which is different from Example 1 in that:
[0161] (1) The raw materials for preparing the silicon-based film etching solution are as follows:
[0162] 450 parts of alkali (potassium hydroxide);
[0163] Surfactant (nonionic surfactant) 5 parts;
[0164] 300 parts of deionized water.
[0165] The parameters of the surfactant used in this example are the same as those in Example 1.
[0166] (2) By weight, the raw materials for preparing the molybdenum-silicon film etching solution are:
[0167]
[0168] The parameters of sulfuric acid and oxidant in this example are the same as those in Example 1.
[0169] Comparative Example 2
[0170] This example etches a phase shift mask, and the specific difference from Example 2 is that:
[0171] (1) The phase shift mask etching solution used is from Comparative Example 1.
[0172] (2) The duration of ultrasonic etching in step S1 is 40 minutes. It can be seen that although the concentration of the alkali is significantly increased compared with Example 2, and the concentration of the surfactant is equivalent, in order to achieve complete etching of the silicon-based film layer, the ultrasonic etching time required in this example is significantly longer than that in Example 1, and the silicon dioxide base layer is obviously damaged.
[0173] In addition, in this example, although the concentration of fluoride in the molybdenum-silicon film etching solution is doubled, the etching speed of the molybdenum-silicon film is still not accelerated. That is to say, compared with Comparative Example 2, although the concentration of fluoride is reduced, Example 2 can still achieve the same technical effect as Example 2.
[0174] Comparative Example 3
[0175] This example etches a phase shift mask, and the specific difference from Example 2 is that:
[0176] In step S1, the temperature of ultrasonic etching is 25°C; within 30 minutes, there is no sign of corrosion on the silicon-based film layer.
[0177] The temperature of ultrasonic etching was raised to 50°C, and the silicon-based film layer gradually corroded after 48 hours.
[0178] It can be seen from this that the corrosion of silicon-based film layers requires a specific temperature range.
[0179] In summary, in the phase-shift mask etching solution provided by the present invention, by adjusting the combination of silicon-based film layer etching solution, chromium-based film layer etching solution and molybdenum-silicon film layer etching solution, the etching rate and etching flatness of the phase-shift mask can be significantly improved on the basis of reducing costs and ensuring stable operation, and the corrosion of the silicon dioxide base layer can be significantly avoided; the rework and stripping problem of the phase-shift mask can be effectively solved.
[0180] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A phase shift mask etching solution, characterized in that: The phase shift mask etching solution includes silicon-based film layer etching solution, chromium-based film layer etching solution and molybdenum-silicon film layer etching solution; The raw materials for preparing the silicon-based film etching solution are as follows: 300-600 parts of alkali; 10-30 parts of surfactant; 400 to 1000 parts of water.
2. The phase shift mask etching solution according to claim 1, characterized in that: The raw materials for preparing the chromium-based film etching solution include, by weight: 100-200 parts of cerium nitrate ammonium; 10-30 parts of acetic acid; 200-800 parts of water.
3. The phase shift mask etching solution according to claim 1, characterized in that: The raw materials for preparing the molybdenum-silicon film etching solution include, by weight:
4. The phase shift mask etching solution according to any one of claims 1 to 3, characterized in that: In the raw materials for preparing the silicon-based film etching solution, the surfactant includes at least one of an anionic surfactant and a non-ionic surfactant.
5. The phase shift mask etching solution according to claim 3, characterized in that: In the raw materials for preparing the molybdenum-silicon film etching solution, the oxidant includes at least one of hydrogen peroxide, periodic acid and sodium hypochlorite; and / or the oxidant is selected from hydrogen peroxide.
6. A method for preparing a phase shift mask etching solution as claimed in any one of claims 1 to 5, characterized in that: include: Mixing the raw materials for preparing the silicon-based film layer etching solution to obtain the silicon-based film layer etching solution; Mixing the raw materials for preparing the chromium-based film layer etching solution to obtain the chromium-based film layer etching solution; The raw materials for preparing the molybdenum-silicon film layer etching solution are mixed to obtain the molybdenum-silicon film layer etching solution.
7. A method for removing a phase-shift mask using the phase-shift mask etching solution according to any one of claims 1 to 5, wherein the phase-shift mask comprises a molybdenum-silicon film layer, a chromium-based film layer and a silicon-based film layer stacked on a silicon dioxide base layer; characterized in that: The method comprises the following steps: S1. The phase shift mask is corroded in the silicon-based film layer etching solution; the etching temperature is 50 to 90°C; S2. The component obtained in step S1 is corroded in the chromium-based film layer in the etching solution; S3. Etching the component obtained in step S2 in the molybdenum-silicon film etching solution.
8. The method according to claim 7, characterized in that In step S1, the corrosion rate is 1-3 μm / min.
9. The method according to claim 7, characterized in that: In step S2, the etching temperature is 20-40°C; and / or, in step S2, the etching rate is 0.2-0.4 μm / min.
10. The method according to claim 7, characterized in that In step S3, the etching temperature is 20-40° C.; and / or, in step S3, the etching rate is 5-10 nm / min.