Production method for improving pouring nodules of high-aluminum non-magnetic steel die casting

By optimizing the electric furnace smelting, LF refining, and IC casting processes for high-alumina non-magnetic steel, the problem of nozzle clogging was solved, enabling smooth casting and efficient production of high-alumina non-magnetic steel.

CN118910356APending Publication Date: 2024-11-08FUSTEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410978880.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the casting process of high-alumina non-magnetic steel, nodules are prone to form at the sprue, which can lead to casting interruption and scrap of molten steel, resulting in serious losses.

Method used

By improving the processes of electric arc furnace smelting, LF refining, and IC casting, including deep slag removal, reducing the amount of refining slag, increasing the casting temperature, using argon protection, and limiting the number of times the ladle is used, the Al2O3 content and impurity accumulation in the molten steel are controlled, and nodule formation at the outlet is avoided.

Benefits of technology

This effectively prevents the formation of lumps at the pouring nozzle, ensuring a smooth pouring process and high-quality molten steel, and reducing production losses.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a production method for improving casting nodules of high-aluminum non-magnetic steel die casting, which sequentially comprises the steps of electric furnace smelting, LF (ladle furnace) refining and IC (integrated circuit) casting, specifically, a product A is obtained through electric furnace smelting, more than 90% of slag in the product A is removed, and then steel is discharged to an LF furnace for LF refining; during LF refining, the content of refining slag added in each ton of the product A is lower than 2.5 Kg, and after LF refining is completed, a product B is obtained; and heating the product B to 1540-1565 DEG C, and carrying out IC casting to obtain a finished product. The product B is heated to 1540-1565 DEG C and then enters a steel ladle to be subjected to IC casting, and the continuous casting use frequency of the steel ladle does not exceed five times; and during IC pouring, argon is adopted for protection, and the argon pressure exceeds 0.11 MPa. The method has the advantage that the nodulation phenomenon of the high-aluminum steel pouring collector nozzle can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-aluminum non-magnetic steel, and in particular relates to a production method for improving die casting nodules of high-aluminum non-magnetic steel. Background Art

[0002] The production method of 18Mn25AlV (C: 0.14-0.22%, Mn: 20.5-25.0%, Al: 1.50-2.50%, V: 0.04-0.30%, Si≤1.0%, P≤0.030%, S≤0.030%) type high-aluminum non-magnetic steel includes electric furnace smelting, LF refining and IC pouring (mold casting) in sequence. In the actual production process, it is found that when the high-aluminum non-magnetic steel is smelted and IC pouring is carried out, the ladle outlet is very prone to nodules. In severe cases, the outlet will be directly blocked, resulting in interruption of pouring and the scrapping of the entire furnace of molten steel, thereby causing serious losses. Summary of the invention

[0003] The purpose of the present invention is to provide a production method for improving the nodule formation during high-aluminum non-magnetic steel die casting. The present invention has the advantage of being able to avoid the nodule formation during casting.

[0004] The technical solution of the present invention is a production method for improving the nodule formation in high-aluminum non-magnetic steel die casting, which comprises the steps of electric furnace smelting, LF refining and IC pouring in sequence. The electric furnace smelting obtains product A, more than 90% of the slag in product A is removed, and the steel is then discharged to the LF furnace for LF refining; during LF refining, the refined slag added to each ton of product A is less than 2.5 kg, and after completing LF refining, product B is obtained; after product B is heated to 1540-1565°C, IC pouring is performed to obtain a finished product.

[0005] In the aforementioned production method for improving high-aluminum non-magnetic steel die casting nodules, the electric furnace smelting, LF refining and IC pouring use the same ladle, and the number of consecutive pouring uses of the ladle does not exceed five times.

[0006] In the above-mentioned production method for improving high-aluminum non-magnetic steel die casting nodules, the temperature of product B is raised to 1540-1565°C before IC casting.

[0007] In the aforementioned production method for improving high-aluminum non-magnetic steel die casting nodules, argon protection is used during IC pouring, and the argon pressure exceeds 0.11MPa.

[0008] In the aforementioned production method for improving high-aluminum non-magnetic steel die casting nodules, the argon pressure is 0.12MPa.

[0009] Compared with the prior art, the present invention mainly makes the following improvements on the basis of the existing production method:

[0010] 1) After smelting in the electric furnace, the amount of slag removal is increased, which greatly reduces the amount of residual slag in the steel strip of the electric furnace, improves the subsequent refining and slag making effect, and allows Al2O3 in the molten steel to enter the slag better, reducing the content of Al2O3 in the molten steel. After a large number of analyses and testing tests, the high content of Al2O3 in the molten steel is an important cause of nodule formation in the water outlet. After reducing the content of Al2O3 in the molten steel, the phenomenon of nodule formation in the water outlet is improved.

[0011] 2) During LF refining, the amount of refining slag is reduced. Since the Al2O3 content in the refining slag used in the LF refining process reaches about 40%, reducing the amount of refining slag can reduce the Al2O3 content in the slag, and the Al2O3 generated in the molten steel can be well floated. After a large number of analyses and testing tests, the addition ratio of existing refining slag is 3.5-6Kg / T, which will lead to a high Al2O3 content in the slag. The Al2O3 inclusions generated in the molten steel during the smelting process cannot be effectively floated, thereby increasing the Al2O3 content in the molten steel, which is easy to cause nodules in the water outlet. After reducing the amount of refining slag to below 2.5Kg / T, the slag adsorption effect is good and the nodule phenomenon in the water outlet is improved.

[0012] 3) The pouring temperature is increased to 1540-1565℃ to avoid nodules at the water outlet caused by the temperature drop of molten steel during the pouring process.

[0013] 4) During pouring, use high pressure argon to protect the molten steel to avoid aluminum oxidation in the molten steel and to prevent the Al2O3 content from increasing again.

[0014] 5) The continuous use times of the ladle are limited to avoid the accumulation of impurities in the ladle.

[0015] After the above five improvements, it was found in the production events of multiple consecutive furnaces that the phenomenon of nodules in the drain nozzle no longer occurred and each furnace was poured smoothly.

[0016] Therefore, the present invention has the advantage of being able to avoid the phenomenon of nodules forming at the pouring nozzle. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0018] Embodiment: A production method for improving high-aluminum non-magnetic steel mold casting nodules, the production object is a 20Mn23AlV type high-aluminum non-magnetic steel mold ingot, which includes electric furnace smelting, LF refining and IC pouring steps in sequence.

[0019] 1) Carbon steel is loaded into the hopper and smelted in an electric furnace to obtain product A. According to conventional operations, carbon blowing and dephosphorization are first performed during smelting to reduce the carbon and phosphorus contents in the molten steel. Aluminum ingots are added for deep deoxidation and electrolytic manganese is added for one time to increase the aluminum and manganese contents to the target range of the steel grade. The aluminum ingots mainly play the role of reducing the molten steel. Finally, product A is tapped with a slag volume of about 1 ton. After tapping and before LF refining, the slag removal volume is changed from conventional slag removal (slag removal volume of about 50%) to deep slag removal, removing more than 90% of the slag volume, making the slag volume less than 100Kg, and then the molten steel is transported to the LF furnace for LF refining.

[0020] Experimental tests have found that there is a causal relationship between the amount of slag removal and the nodule formation during pouring. Deep slag removal can improve the slag-making effect during subsequent LF refining, thereby reducing the alumina content in molten steel and improving the nodule formation phenomenon at the pouring nozzle.

[0021] 2) During LF refining, according to the normal operation, lime, fluorite and refining slag are added to product A for slagging. The amount of lime added is maintained at a normal amount of 20kg per ton of product A, and the amount of fluorite added is maintained at a normal amount of 10kg per ton of product A. The amount of refining slag added is reduced from 3.5-6kg per ton of product A to less than 2.5Kg, such as 1.6Kg. Aluminum ingots and electrolytic manganese are added by one main addition and one or two fine adjustments to adjust the internal composition of the molten steel. After completing LF refining, product B is obtained.

[0022] After multiple tests, the Al2O3 content in the furnace slag of the down-flow nodule is about 30%, while the Al2O3 content in the furnace slag of the normal pouring is less than 25%. When the Al2O3 in the refining slag reaches about 40%, the Al2O3 content in the slag will be greatly increased, and the Al2O3 generated in the molten steel cannot float well. Therefore, during LF refining, by reducing the amount of refining slag, it is ensured that the slag has enough distribution ratio (theoretical index of the adsorption capacity of Al2O3) for Al2O3, so that the Al2O3 generated in the molten steel smelting process can float well in the slag. When the amount of refining slag is 1.6Kg / ton of steel, the slag-making effect remains good and the slag has a good Al2O3 adsorption effect.

[0023] 3) Product B is heated to 1540-1565℃ and cast in IC. During IC casting, argon protection is used. The argon pressure exceeds 0.11MPa, preferably 0.12MPa. Exceeding 0.12MPa will lead to waste of argon and obtain the finished product. The same ladle is used for electric furnace smelting, LF refining and IC casting. The ladle is used for continuous casting for no more than five times.

[0024] It was found through experiments that, first, under the existing production method, the pouring temperature is 1500-1525℃, and the temperature drop during the pouring process will cause nodules at the water outlet. Therefore, it is necessary to increase the pouring temperature to 1540-1565℃, which can significantly improve the nodule phenomenon caused by the temperature drop of the molten steel during the pouring process. Second, under the existing production method, the ladle is used continuously, and during the production process, the ladle wall and the bottom of the ladle are difficult to clean, which makes the impurities in the ladle increase continuously. Therefore, the ladle is replaced every time 5 furnaces of this type of steel are smelted continuously to ensure that the ladle is clean and free of impurities and does not affect normal smelting. This also plays a positive role in avoiding nodules at the water outlet. Third, due to the high aluminum content in the molten steel, it is very easy to produce secondary oxidation when mixed with air during pouring, so argon protection is used during the pouring process, and the pressure needs to exceed 0.11MPa, with about 0.12MPa being the best. When the pressure drops to 0.1MPa, nodules are easy to occur.

Claims

1. A production method for improving high-aluminum non-magnetic steel die casting nodules, comprising the steps of electric furnace smelting, LF refining and IC pouring, characterized in that: Product A is obtained by electric furnace smelting, and more than 90% of the slag in product A is removed, and then the steel is tapped into the LF furnace for LF refining; during LF refining, the refined slag added to each ton of product A is less than 2.5 kg, and after LF refining, product B is obtained; after product B is heated to 1540-1565℃, IC pouring is carried out to obtain the finished product.

2. The production method for improving high-aluminum non-magnetic steel die casting nodules according to claim 1 is characterized in that: The same ladle is used for electric furnace tapping, LF refining and IC pouring, and the ladle shall not be used for continuous pouring more than five times.

3. The production method for improving high-aluminum non-magnetic steel die casting nodules according to claim 1, characterized in that: Product B is heated to 1540-1565℃ before IC pouring.

4. The production method for improving high-aluminum non-magnetic steel die casting nodules according to claim 1, characterized in that: When IC is poured, argon protection is used and the argon pressure exceeds 0.11MPa.

5. The production method for improving high-aluminum non-magnetic steel die casting nodules according to claim 4 is characterized in that: Argon pressure: 0.12MPa.