Fluorine-free oil-proof agent and production method of oil-proof paper
Through the fluorine-free oil-proofing agent and multi-layer coating process that synergistically acts sodium alginate and hydroxypropylmethylcellulose, the environmental and health risks of traditional oil-proof paper are solved, and high-performance, environmentally friendly fluorine-free oil-proof paper production is achieved. Suitable for the food packaging industry.
Patent Information
- Application Number
- CN202411202550.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional fluorine-containing compounds of oil-resistant paper have environmental and health risks. The existing fluorine-free oil-resistant agents have insufficient oil-resistant performance, high cost or complex production process, and poor physical performance indicators.
The fluorine-free oil-proofing agent that synergistically acts by sodium alginate and hydroxypropylmellose is used, combined with specific slurry ratio and multi-layer coating process, optimize the base paper preparation process and improve the mechanical strength and oil-proof performance of oil-proof paper.
Developed biodegradable, environmentally friendly fluorine-free oil-resistant paper with good oil-resistant properties, mechanical strength and physical performance indicators, and is suitable for the food packaging industry, especially in the fast food industry and baked food packaging.
Smart Images

Figure CN118910909A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of oil-proof paper production, and particularly relates to a fluorine-free oil-proof agent and a production method of oil-proof paper. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] As people's awareness of food safety and environmental protection increases, the demand for grease-proof paper is growing. Grease-proof paper is widely used in the food packaging industry, especially in the fast food industry and baked food packaging.
[0004] Traditional oil-proof paper usually uses fluorinated compounds as oil-proof agents. Although these compounds have good oil-proof properties, they have attracted more and more attention due to their potential environmental and health risks. Fluorinated compounds (such as perfluoroalkyl substances PFAS) are difficult to degrade and exist in the environment for a long time, which may cause adverse effects on human health. Therefore, finding safer and more environmentally friendly alternatives has become an important direction of current research.
[0005] There are already some fluorine-free oil-proofing agents on the market, but they often have problems such as insufficient oil-proofing performance, high cost, poor physical performance indicators or complex production process. For example, although the chitosan and sodium alginate compound oil-proofing agent can achieve an oil-proofing effect similar to that of the fluorine-containing oil-proofing agent, it is not conducive to large-scale application due to its high cost and high viscosity during the processing process. The physical properties of the oil-proof paper produced by coating with conventional paper are insufficient, such as low tensile strength and smoothness.
[0006] Hydroxypropyl methylcellulose (HPMC), as a biodegradable polymer material, has been widely used in many fields, including pharmaceuticals, cosmetics and personal care products. HPMC has good film-forming properties and stability, but its oil-proof performance is limited when used alone as an oil-proof agent.
[0007] Therefore, it is urgent to overcome the problems existing in the existing oil-proof paper, such as poor oil-proof performance and poor physical performance indicators. Summary of the invention
[0008] In order to solve the above problems, the present invention provides a fluorine-free oil-proof agent and a method for producing oil-proof paper. By developing a new fluorine-free oil-proof agent, optimizing the base paper preparation process, the wet-end chemical formulation and the multi-layer coating process, the production of fluorine-free, environmentally friendly and degradable oil-proof paper is achieved, and the mechanical strength of the oil-proof paper is improved.
[0009] In order to achieve the above object, the present invention adopts the following technical solution:
[0010] The first aspect of the present invention provides a fluorine-free oil repellent, comprising: a solution A and a solution B, wherein the volume ratio of the solution A to the solution B is 1:0.3-0.5;
[0011] The solution A is a sodium alginate solution, which is composed of the following raw materials in percentage by mass: 1-2% sodium alginate, 2-3% glycerol, and the rest water;
[0012] The solution B is a hydroxypropyl methylcellulose solution, which is composed of the following raw materials in percentage by mass: 2-3% hydroxypropyl methylcellulose, 2-3% glycerol, and the remainder water.
[0013] Research has found that sodium alginate is a natural polysaccharide with a wide range of sources and good biocompatibility and degradability. It can work synergistically with hydroxypropyl methylcellulose, calcium ions, etc. to improve the overall performance of oil repellents.
[0014] The second aspect of the present invention provides a method for preparing a fluorine-free oil-proofing agent, comprising:
[0015] Mix sodium alginate, water and glycerol evenly to obtain a sodium alginate solution, which is referred to as solution A;
[0016] Mixing hypromellose, water and glycerin uniformly to obtain a hypromellose solution, which is referred to as solution B;
[0017] The solution A and the solution B are mixed evenly to obtain a fluorine-free oil repellent.
[0018] In some embodiments, the sodium alginate has a viscosity of 40-60 cps, a dissolution temperature of 60-70° C., and a dissolution time of 30-60 min;
[0019] In some embodiments, the viscosity of the hypromellose is 6-10 cps, the dissolution temperature is 80-90° C., and the dissolution time is 30-60 min;
[0020] In some embodiments, the mixing temperature of solution A and solution B is 65-75° C., and the mixing time is 30-60 min.
[0021] A third aspect of the present invention provides a method for producing oil-proof paper, comprising:
[0022] Mixing coniferous chemical pulp, broadleaf chemical pulp, poplar chemical mechanical pulp, filler, cationic starch, retention aid, brightener, and neutral glue uniformly to obtain slurry, and using the slurry to prepare base paper;
[0023] The pigment, adhesive, water repellent, rheological agent, thickener, defoamer and bactericide are mixed evenly to prepare a primer, and the base paper is coated with the primer once;
[0024] Using CaCl2 solution as coating, the paper coated with the first bottom layer is subjected to a second bottom layer coating;
[0025] The above-mentioned fluorine-free oil-proofing agent is used to coat the surface layer of the paper after the secondary bottom layer coating to obtain the paper.
[0026] It should be noted that the present invention does not specifically limit the pulp raw materials, preparation processes, etc. of coniferous chemical pulp, broadleaf chemical pulp, and poplar chemical mechanical pulp. The above pulps only need to meet the requirements of beating degree and beating concentration to meet the production requirements of base paper and oil-proof paper of the present invention. Therefore, in some embodiments, the coniferous chemical pulp has a beating degree of 43-47°SR and a beating concentration of 3.9-4.2%;
[0027] In some embodiments, the broadleaf chemical pulp has a beating degree of 28-32°SR and a beating concentration of 3.8-4.3%;
[0028] In some embodiments, the poplar chemical mechanical pulp has a beating degree of 35-37° SR and a beating concentration of 3.4-3.6%.
[0029] In some embodiments, the ratio of coniferous chemical pulp, broadleaf chemical pulp, and poplar chemical mechanical pulp is 20-30:50-60:20-30;
[0030] In some embodiments, the filler is light calcium, nano calcium and diatomaceous earth; the weight ratio of the light calcium, nano calcium and diatomaceous earth is 3-4:1:1, the filler concentration is 14-16%, and the dosage is 190-210 kg / ton of paper;
[0031] It should be noted that "filler concentration of 14-16%" means: the filler is prepared into a solution with a concentration of 14-16% and then added to the slurry. The concentrations of cationic starch, retention aid, brightener and neutral gum have the same meaning.
[0032] In some embodiments, the concentration of the cationic starch is 2-3%, and the dosage is 10-11 kg / ton of paper;
[0033] In some embodiments, the retention aid is cationic polyacrylamide or polyethyleneimine or polydimethyldiallylammonium chloride, with a concentration of 2.3-2.7% and an amount of 0.2-0.3 kg / ton of paper;
[0034] In some embodiments, the brightener is one of tetrasulfonic acid or hexasulfonic acid, and the dosage is 3-3.5 kg / ton of paper;
[0035] In some embodiments, the neutral glue is AKD or cationic rosin glue, the concentration of AKD is 15%, the concentration of cationic rosin glue is 35%, and the dosage is 10-15 kg / ton of paper.
[0036] In some embodiments, the primer is composed of the following raw materials in parts by weight: 100 parts of pigment, 10-12 parts of adhesive, 0.4-0.6 parts of water repellent, 0.4-0.6 parts of rheological agent, 0.4-0.6 parts of thickener, 0.1-0.2 parts of defoamer, and 0.1-0.2 parts of fungicide;
[0037] In some embodiments, the pigment is light calcium or china clay;
[0038] In some embodiments, the adhesive is carboxylated styrene butadiene latex or acrylic emulsion;
[0039] In some embodiments, the water repellent is potassium zirconium carbonate, modified glyoxal, polyamide polyurea or ammonium zirconium carbonate;
[0040] In some embodiments, the rheological agent is modified acrylic acid;
[0041] In some embodiments, the thickener is polyurethane emulsion, carboxymethyl cellulose, hydroxyethyl cellulose, polyvinyl alcohol or polyacrylamide;
[0042] In some embodiments, the defoaming agent is polyether, C18-C20 higher fatty alcohol or silicone;
[0043] In some embodiments, the bactericide is an organic bromine;
[0044] In some embodiments, the coating weight of a primer coating is 5-6 g / m 2 .
[0045] In some embodiments, the concentration of the CaCl2 solution is 3-4%;
[0046] In some embodiments, the secondary bottom layer coating is applied by air knife coating with a coating amount of 2-4 g / m 2 .
[0047] In some embodiments, the surface coating method is blade coating, and the coating amount is controlled to be 4-6 g / m 2 , coating temperature 60-65℃.
[0048] A fourth aspect of the present invention provides oil-proof paper prepared by the above method.
[0049] The fifth aspect of the present invention provides the use of the above-mentioned fluorine-free oil-proof agent and the above-mentioned oil-proof paper in the food packaging industry, especially in the fast food industry and baked food packaging.
[0050] Beneficial effects of the present invention
[0051] (1) The oil-proofing agent of the present invention does not contain fluorine and is mainly derived from sodium alginate and hydroxypropyl methylcellulose, which are made from brown algae and cellulose, respectively, and are biodegradable.
[0052] (2) The method for producing oil-proof paper of the present invention uses a specific pulp ratio, a specific coating material of the coating layer and a coating process to obtain paper having not only good oil-proof performance but also good bulk, whiteness and mechanical strength.
[0053] (3) The basis weight of the oil-proof paper of the present invention is 58-63 g / m 2 , whiteness 80-84% ISO, opacity>85%, smoothness 105-115s, transverse tensile strength 1.8-1.9kN / m, longitudinal tensile strength 3.7-4.0kN / m, oil proof grade ≥9.
[0054] (4) The preparation method of the present invention is simple, practical and easy to promote. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention, and the exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute improper limitations on the present invention.
[0056] Figure 1 These are SEM images of base paper, comparative example 1, and paper of example 2. DETAILED DESCRIPTION
[0057] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0058] It should be noted that, in the present invention, unless otherwise specified, concentrations are all mass concentrations.
[0059] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.
[0060] Embodiment 1:
[0061] Preparation of fluorine-free oil repellent:
[0062] Sodium alginate, water and glycerol are mixed and stirred evenly to obtain a sodium alginate solution (solution A); hydroxypropyl methylcellulose, water and glycerol are mixed and stirred evenly to obtain a hydroxypropyl methylcellulose solution (solution B); solution A and solution B are mixed and stirred evenly to obtain a fluorine-free oil-proofing agent.
[0063] The mass concentration of the sodium alginate solution (solution A) is 1%, the mass concentration of glycerol is 2%, and the rest is water. The viscosity of the sodium alginate is 40-60 cps, the dissolution temperature is 70° C., and the dissolution time is 30 min.
[0064] The mass concentration of the hydroxypropyl methylcellulose solution (solution B) is 2%, the concentration of glycerol is 2%, the viscosity of the hydroxypropyl methylcellulose is 6-10 cps, the dissolution temperature is 80° C., and the dissolution time is 30 min.
[0065] In the fluorine-free oil repellent, the ratio of solution A to solution B is 1:0.3, the mixing temperature is 65° C., and the mixing time is 30 min.
[0066] Preparation of base paper:
[0067] The base paper is prepared by uniformly mixing coniferous chemical pulp, broadleaf chemical pulp, poplar chemical mechanical pulp, filler, cationic starch, retention aid, brightener and neutral glue.
[0068] The coniferous chemical pulp has a beating degree of 43°SR and a beating concentration of 3.9%.
[0069] The broadleaf chemical pulp has a beating degree of 28°SR and a beating concentration of 3.8%.
[0070] The poplar chemical mechanical pulp has a beating degree of 35°SR and a beating concentration of 3.46%.
[0071] The ratio of the coniferous chemical pulp, the broadleaf chemical pulp and the poplar chemical mechanical pulp is 20:50:30.
[0072] The filler is light calcium, nano calcium and diatomaceous earth; the weight ratio of the light calcium, nano calcium and diatomaceous earth is 3:1:1, the filler concentration is 14%, and the dosage is 190kg / ton of paper.
[0073] The concentration of the cationic starch is 2%, and the dosage is 10 kg / ton of paper.
[0074] The retention aid is cationic polyacrylamide, with a concentration of 2.4% and a dosage of 0.2 kg / ton of paper.
[0075] The brightener is tetrasulfonic acid, and the dosage is 3kg / ton of paper.
[0076] The neutral glue is AKD, the concentration of AKD is 15%, and the dosage is 10kg / ton of paper.
[0077] One-time base coating:
[0078] The base paper prepared above was coated with a bottom layer by blade coating, and the coating amount was controlled to be 5g / m 2 The coating formula is pigment, adhesive, water repellent, rheological agent, thickener, defoamer, bactericide. The formula ratio is calculated as follows:
[0079] Pigment: adhesive: water repellent: rheological agent: thickener: defoamer: bactericide = 100:10:0.4:0.6:0.4:0.1:0.2.
[0080] The pigment is light calcium.
[0081] The adhesive is carboxyl styrene butadiene latex.
[0082] The water repellent is potassium zirconium carbonate.
[0083] The rheological agent is ethyl methacrylate.
[0084] The thickener is polyacrylamide.
[0085] The defoamer is polyether;
[0086] The bactericide is organic bromine.
[0087] Secondary base coating:
[0088] The paper coated with the primary bottom layer was subjected to secondary bottom layer coating. The coating was a CaCl2 solution with a concentration of 3%. The coating was performed by air knife coating with a coating amount of 3 g / m 2 .
[0089] Surface coating:
[0090] The paper after the secondary bottom coating is coated with a surface coating, the coating is a fluorine-free oil-proof agent, and the coating amount is 5g / m 2 , coating temperature is 60℃, and coating method is blade coating.
[0091] Embodiment 2:
[0092] Preparation of fluorine-free oil repellent:
[0093] Sodium alginate, water and glycerol are mixed and stirred evenly to obtain a sodium alginate solution (solution A); hydroxypropyl methylcellulose, water and glycerol are mixed and stirred evenly to obtain a hydroxypropyl methylcellulose solution (solution B); solution A and solution B are mixed and stirred evenly to obtain a fluorine-free oil-proofing agent.
[0094] The mass concentration of the sodium alginate solution (solution A) is 2%, the mass concentration of glycerol is 3%, and the rest is water. The viscosity of the sodium alginate is 40-60 cps, the dissolution temperature is 70° C., and the dissolution time is 60 min.
[0095] The mass concentration of the hydroxypropyl methylcellulose solution (solution B) is 3%, the concentration of glycerol is 2%, the viscosity of the hydroxypropyl methylcellulose is 6-10 cps, the dissolution temperature is 90° C., and the dissolution time is 60 min.
[0096] In the fluorine-free oil repellent, the ratio of solution A to solution B is 1:0.5, the mixing temperature is 75° C., and the mixing time is 60 min.
[0097] Preparation of base paper:
[0098] The base paper is prepared by uniformly mixing coniferous chemical pulp, broadleaf chemical pulp, poplar chemical mechanical pulp, filler, cationic starch, retention aid, brightener and neutral glue.
[0099] The coniferous chemical pulp has a beating degree of 47°SR and a beating concentration of 4%.
[0100] The broadleaf chemical pulp has a beating degree of 32°SR and a beating concentration of 4%.
[0101] The poplar chemical mechanical pulp has a beating degree of 37°SR and a beating concentration of 3.6%.
[0102] The ratio of coniferous chemical pulp, broadleaf chemical pulp and poplar chemical mechanical pulp is 25:45:30.
[0103] The filler is light calcium, nano calcium and diatomaceous earth; the weight ratio of the light calcium, nano calcium and diatomaceous earth is 3.5:1:1, the filler concentration is 16%, and the dosage is 210kg / ton of paper.
[0104] The concentration of the cationic starch is 3%, and the dosage is 11 kg / ton of paper.
[0105] The retention aid is polydimethyldiallylammonium chloride, with a concentration of 2.7% and a dosage of 0.3 kg / ton of paper.
[0106] The brightener is hexasulfonic acid, and the dosage is 3kg / ton of paper.
[0107] The neutral glue is cationic rosin glue, the concentration of the cationic rosin glue is 35%, and the usage is 12kg / ton of paper.
[0108] One-time base coating:
[0109] The base paper prepared above was coated with a bottom layer by blade coating, and the coating amount was controlled to be 5.3 g / m 2The coating formula is pigment, adhesive, water repellent, rheological agent, thickener, defoamer, and bactericide. The formula ratio is calculated on an absolute dry basis:
[0110] Pigment: adhesive: water repellent: rheological agent: thickener: defoamer: bactericide = 100:112:0.6:0.4:0.6:0.1:0.2.
[0111] The pigment is china clay.
[0112] The adhesive is acrylic emulsion.
[0113] The water repellent is ammonium zirconium carbonate.
[0114] The rheological agent is ethyl methacrylate.
[0115] The thickener is carboxymethyl cellulose.
[0116] The defoaming agent is cetearyl alcohol;
[0117] The bactericide is organic bromine.
[0118] The secondary bottom coating:
[0119] The paper coated with the primary bottom layer was coated with the secondary bottom layer, and the coating amount was 3.6 g / m 2 The coating is a CaCl2 solution with a concentration of 4%, which is applied by air knife coating.
[0120] The surface coating:
[0121] The paper after the secondary bottom coating is coated with a surface coating, the coating is a fluorine-free oil-proofing agent, and the coating amount is 4.8g / m 2 , coating temperature is 65℃, and coating method is blade coating.
[0122] Embodiment 3:
[0123] Preparation of fluorine-free oil repellent:
[0124] Sodium alginate, water and glycerol are mixed and stirred evenly to obtain a sodium alginate solution (solution A); hydroxypropyl methylcellulose, water and glycerol are mixed and stirred evenly to obtain a hydroxypropyl methylcellulose solution (solution B); solution A and solution B are mixed and stirred evenly to obtain a fluorine-free oil-proofing agent.
[0125] The mass concentration of the sodium alginate solution (solution A) is 1.5%, the mass concentration of glycerol is 3%, and the rest is water. The viscosity of the sodium alginate is 40-60 cps, the dissolution temperature is 65° C., and the dissolution time is 50 min.
[0126] The mass concentration of the hydroxypropyl methylcellulose solution (solution B) is 2.5%, the concentration of glycerol is 3%, the viscosity of the hydroxypropyl methylcellulose is 6-10 cps, the dissolution temperature is 85° C., and the dissolution time is 45 min.
[0127] In the fluorine-free oil repellent, the ratio of solution A to solution B is 1:0.4, the mixing temperature is 70° C., and the mixing time is 50 min.
[0128] Preparation of base paper:
[0129] The base paper is prepared by uniformly mixing coniferous chemical pulp, broadleaf chemical pulp, poplar chemical mechanical pulp, filler, cationic starch, retention aid, brightener and neutral glue.
[0130] The coniferous chemical pulp has a beating degree of 45°SR and a beating concentration of 4%.
[0131] The broadleaf chemical pulp has a beating degree of 30°SR and a beating concentration of 4%.
[0132] The poplar chemical mechanical pulp has a beating degree of 35-37°SR and a beating concentration of 3.5%.
[0133] The ratio of the coniferous chemical pulp, the broadleaf chemical pulp and the poplar chemical mechanical pulp is 30:50:20.
[0134] The filler is light calcium, nano calcium and diatomaceous earth; the weight ratio of the light calcium, nano calcium and diatomaceous earth is 3.5:1:1, the filler concentration is 15%, and the dosage is 200kg / ton of paper.
[0135] The concentration of the cationic starch is 2.5%, and the dosage is 10.5 kg / ton of paper.
[0136] The retention aid is cationic polyacrylamide, with a concentration of 2.5% and a dosage of 0.25 kg / ton of paper.
[0137] The brightener is tetrasulfonic acid, and the dosage is 3.3 kg / ton of paper.
[0138] The neutral glue is AKD, the concentration of AKD is 15%, and the dosage is 13kg / ton of paper.
[0139] One-time base coating:
[0140] The base paper prepared above was coated with a bottom layer by blade coating, and the coating amount was controlled to be 5.5 g / m 2 The coating formula is pigment, adhesive, water repellent, rheological agent, thickener, defoamer, bactericide. The formula ratio is calculated as follows:
[0141] Pigment: adhesive: water repellent: rheological agent: thickener: defoamer: bactericide = 100:112:0.6:0.4:0.6:0.1:0.2.
[0142] The pigment is china clay.
[0143] The adhesive is acrylic emulsion.
[0144] The water repellent is ammonium zirconium carbonate.
[0145] The rheological agent is ethyl methacrylate.
[0146] The thickener is carboxymethyl cellulose.
[0147] The defoaming agent is cetearyl alcohol;
[0148] The bactericide is organic bromine.
[0149] The secondary bottom coating:
[0150] The paper coated with the primary bottom layer was coated with the secondary bottom layer, and the coating amount was 2.4g / m 2 The coating is a CaCl2 solution with a concentration of 4%, which is applied by air knife coating.
[0151] The surface coating:
[0152] The paper after the secondary bottom coating is coated with a surface coating, the coating is a fluorine-free oil-proofing agent, and the coating amount is 5.4g / m 2 , coating temperature is 65℃, and coating method is blade coating.
[0153] Comparative Example 1:
[0154] The secondary bottom coating in Example 1 was omitted, and the other steps were the same as in Example 1 to obtain paper.
[0155] Comparative Example 2:
[0156] The surface coating in Example 1 was omitted, and the other steps were the same as in Example 1 to obtain paper.
[0157] Experimental Example 1:
[0158] The paper obtained in the embodiment and the comparative example was subjected to performance tests, and the test results are shown in Table 1:
[0159] Table 1 Paper performance test results
[0160]
[0161]
[0162] The base paper, the comparative example 1, and the paper of Example 2 were observed by SEM. Figure 1 shown.
[0163] It can be seen from Table 1 that the oil-proof grades in Examples 1, 2 and 3 are all over Grade 8, while the oil-proof grades in Comparative Examples 1 and 2 are lower. This is mainly because the calcium chloride solution coating is omitted in Comparative Example 1, and only the fluorine-free oil-proof agent is coated. Although it has a certain oil-proof effect, sodium alginate cannot cross-link with calcium ions, resulting in a decrease in the oil-proof effect; and in Comparative Example 2, no oil-proof agent is added, and only the wet-end additive added by the primary bottom coating is relied on, so the oil-proof effect is poor.
[0164] From the SEM images of the paper, the surface morphologies of the base paper, comparative example 1 and example 2 can be observed. The surface of the uncoated base paper shows obvious fibers and fillers, and there are a large number of gaps between the fibers. In comparative example 1, the fiber texture can still be seen, but the surface of the paper begins to become smooth, with a certain oil-proof effect. In example 2, the fibers on the surface of the paper are almost completely covered, the surface becomes smoother, and grease is difficult to penetrate, so it has a better oil-proof grade.
[0165] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A fluorine-free oil-proofing agent, characterized in that: include: Solution A and solution B, wherein the volume ratio of solution A to solution B is 1:0.3-0.5; The solution A is a sodium alginate solution, which is composed of the following raw materials in percentage by mass: 1-2% sodium alginate, 2-3% glycerol, and the rest water; The solution B is a hydroxypropyl methylcellulose solution, which is composed of the following raw materials in percentage by mass: 2-3% hydroxypropyl methylcellulose, 2-3% glycerol, and the remainder water.
2. A method for preparing a fluorine-free oil-proofing agent, characterized in that: include: Mix sodium alginate, water and glycerol evenly to obtain a sodium alginate solution, which is referred to as solution A; Mixing hypromellose, water and glycerin uniformly to obtain a hypromellose solution, which is referred to as solution B; The solution A and the solution B are mixed evenly to obtain a fluorine-free oil repellent.
3. The method for preparing the fluorine-free oil-proofing agent according to claim 2, characterized in that: The sodium alginate has a viscosity of 40-60 cps, a dissolution temperature of 60-70°C, and a dissolution time of 30-60 min; Or, the viscosity of the hypromellose is 6-10 cps, the dissolution temperature is 80-90° C., and the dissolution time is 30-60 min; Alternatively, the mixing temperature of the solution A and the solution B is 65-75° C., and the mixing time is 30-60 min.
4. A method for producing oil-proof paper, characterized in that: include: Mixing coniferous chemical pulp, broadleaf chemical pulp, poplar chemical mechanical pulp, filler, cationic starch, retention aid, brightener, and neutral glue uniformly to obtain slurry, and using the slurry to prepare base paper; The pigment, adhesive, water repellent, rheological agent, thickener, defoamer and bactericide are mixed evenly to prepare a primer, and the base paper is coated with the primer once; Using CaCl2 solution as coating, the paper coated with the first bottom layer is subjected to a second bottom layer coating; The non-fluorinated oil-proofing agent according to claim 1 is used to coat the surface of the paper after secondary bottom coating to obtain the paper.
5. The method for producing oil-proof paper according to claim 4, characterized in that: The coniferous chemical pulp has a beating degree of 43-47°SR and a beating concentration of 3.9-4.2%; Or, the broadleaf chemical pulp has a beating degree of 28-32°SR and a beating concentration of 3.8-4.3%; Alternatively, the poplar chemical mechanical pulp has a beating degree of 35-37° SR and a beating concentration of 3.4-3.6%. Or, the ratio of coniferous chemical pulp, broadleaf chemical pulp and poplar chemical mechanical pulp is 20-30:50-60:20-30; Or, the filler is light calcium, nano calcium and diatomaceous earth; the weight ratio of the light calcium, nano calcium and diatomaceous earth is 3-4:1:1, the filler concentration is 14-16%, and the dosage is 190-210 kg / ton of paper; Or, the concentration of the cationic starch is 2-3%, and the dosage is 10-11 kg / ton of paper; Or, the retention aid is cationic polyacrylamide or polyethyleneimine or polydimethyldiallylammonium chloride, with a concentration of 2.3-2.7% and a dosage of 0.2-0.3 kg / ton of paper; Or, the brightener is one of tetrasulfonic acid or hexasulfonic acid, and the dosage is 3-3.5 kg / ton of paper; Or, the neutral glue is AKD or cationic rosin glue, the concentration of AKD is 15%, the concentration of cationic rosin glue is 35%, and the dosage is 10-15kg / ton of paper.
6. The method for producing oil-proof paper according to claim 4, characterized in that: The primer is composed of the following raw materials in parts by weight: 100 parts of pigment, 10-12 parts of adhesive, 0.4-0.6 parts of water repellent, 0.4-0.6 parts of rheological agent, 0.4-0.6 parts of thickener, 0.1-0.2 parts of defoamer, and 0.1-0.2 parts of bactericide; Or, the pigment is light calcium or china clay; Or, the adhesive is carboxylated styrene-butadiene latex or acrylic emulsion; Or, the water repellent is potassium zirconium carbonate, modified glyoxal, polyamide polyurea or ammonium zirconium carbonate; Or, the rheological agent is modified acrylic acid; Or, the thickener is polyurethane emulsion, carboxymethyl cellulose, hydroxyethyl cellulose, polyvinyl alcohol or polyacrylamide; Or, the defoamer is polyether, C18-C20 higher fatty alcohol or silicone; Or, the bactericide is an organic bromine; Or, the coating amount of the base coating is 5-6g / m 2 .
7. The method for producing oil-proof paper according to claim 4, characterized in that: The concentration of the CaCl2 solution is 3-4%; Alternatively, the secondary base coating is applied by air knife coating with a coating weight of 2-4 g / m 2 .
8. The method for producing oil-proof paper according to claim 6, characterized in that: The surface coating method is scraper coating, and the coating amount is controlled to be 4-6g / m 2 , coating temperature 60-65℃.
9. Oil-proof paper prepared by the method according to any one of claims 4 to 8.
10. Use of the fluorine-free oil-proof agent according to claim 1 and the oil-proof paper according to claim 9 in the food packaging industry.
Citation Information
Patent Citations
Sizing composition for fluoride-free food paper as well as preparation method and application of sizing composition
CN114855504A
Bio-based waterproof and oilproof packaging paper and preparation method thereof
CN114990936A
Bio-based Waterproof and Oil-proof Wrapping Paper and Preparation Method Thereof
US20230323602A1