Uranium nitride nuclear fuel pellet and preparation method thereof

Through hydrogenated dehydrogenation and high-purity nitrogen treatment, combined with vacuum sintering technology, a high-density uranium nitride nuclear fuel core pellet was prepared, which solved the problem of swelling and deformation of uranium nitride nuclear fuel under irradiation conditions and achieved high irradiation stability. Suitable for nuclear reactors.

CN118919112APending Publication Date: 2024-11-08SHANGHAI INSTITUTE OF APPLIED PHYSICS CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202410968256.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Uranium nitride nuclear fuel will produce high swelling and deformation under irradiation conditions, limiting its application in nuclear reactors.

Method used

The uranium block is prepared into uranium powder by hydrogenation dehydrogenation, and heats up to form the first powder in a heating furnace of high-purity nitrogen or nitrogen and inert gas. Then sintered in a vacuum air atmosphere, controlling the heating rate and insulation time to form a high-volume Density of uranium nitride nuclear fuel pellets.

Benefits of technology

The prepared uranium nitride nuclear fuel pellet has high density and high irradiation stability, and does not expand after irradiation, and is suitable for new nuclear fuels for nuclear reactors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919112A_ABST
    Figure CN118919112A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a uranium nitride nuclear fuel pellet. The preparation method comprises the following steps: preparing uranium blocks into uranium powder through hydrogenation dehydrogenation; the uranium powder is placed in a heating furnace into which high-purity nitrogen or mixed gas of nitrogen and inert gas is introduced for heating and heat preservation, first powder is formed along with furnace cooling, and the first powder is pressed into a first green body; placing the first green body in a high-temperature heating furnace in a vacuum atmosphere for heating and heat preservation, and cooling along with the furnace to obtain a second green body; the second green body is made into second powder, and the second powder is pressed into a third green body; and the third blank is placed in a high-temperature rapid sintering furnace in a vacuum atmosphere, temperature rise and heat preservation are carried out, constant pressure is axially applied to the third blank, and the uranium nitride nuclear fuel pellet is prepared through sintering. The uranium nitride nuclear fuel pellet provided by the invention is obtained according to the preparation method. The uranium nitride nuclear fuel pellet prepared by the preparation method has the advantages of high density and high irradiation stability, and can be used as a novel nuclear fuel of a nuclear reactor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to nuclear power technology, and more specifically to a uranium nitride nuclear fuel pellet and a preparation method thereof. Background Art

[0002] Compared with UO2 fuel widely used in commercial reactors, uranium nitride fuel has the advantages of both metal fuel and oxide fuel. It has high thermal conductivity and high metal atom density like metal fuel, and high melting temperature and isotropic crystal structure like oxide fuel. Its high thermal conductivity and high melting temperature can achieve high linear power operation; and large diameter fuel plugs can be used at a given linear power. Due to its high metal atom density, it can accommodate a certain amount of fission products, while achieving flexible core design and high neutron economy, thereby further improving fuel cycle time. These characteristics make uranium nitride nuclear fuel an important candidate fuel for future space reactor power and the fourth-generation nuclear energy system lead-cooled fast reactor (LCR) and sodium-cooled fast reactor (SCFR).

[0003] However, the application of uranium nitride nuclear fuel pellets in nuclear reactors is limited because nitride nuclear fuel will produce higher swelling deformation and swelling rate under irradiation conditions. Summary of the invention

[0004] In order to solve the problem that the nitride nuclear fuel in the prior art will produce high swelling and deformation under irradiation conditions, the present invention provides a uranium nitride nuclear fuel pellet and a preparation method thereof.

[0005] The preparation method of uranium nitride nuclear fuel pellets according to the present invention comprises the following steps: S1, preparing uranium blocks (also called uranium ingots) into uranium powder by hydrogenation and dehydrogenation; S2, placing the uranium powder in a heating furnace into which high-purity nitrogen or a mixture of nitrogen and inert gas is introduced, heating the uranium powder to 300° C. to 600° C. at a rate of 5 to 10° C. / min, keeping the temperature for 3 to 8 hours, cooling the powder along with the furnace to form a first powder, and then pressing the first powder into a first blank under a pressure of 4 to 9 tons; S3, placing the first blank in a high-temperature heating furnace in a vacuum atmosphere, heating the first blank to 250 to 350° C. at a rate of 10 to 30° C. / min, and heating the first blank to 350 to 350° C. 0℃, then raise the temperature to 1300-1600℃ at a speed of 10-30℃ / min, keep warm for 1-5h, cool with the furnace to obtain a second green body; S4, make the second green body into a second powder with a size of 10-25 microns, and then press the second powder into a third green body under a pressure of 4-9 tons; S5, place the third green body in a high-temperature rapid sintering furnace in a vacuum atmosphere, raise the temperature to 1400-1600℃ at a speed of 90-110℃ / min, keep warm for 5-20min, apply a constant pressure of 30-50MPa to the axial direction of the third green body, and sinter to obtain uranium nitride nuclear fuel pellets.

[0006] In a preferred embodiment, step S1 comprises: externally using concentrated nitric acid and anhydrous ethanol to clean the surface of the uranium block, grinding and polishing in a glove box to remove the surface oxide, then putting the uranium block into a tungsten crucible, placing it in a closed high-temperature furnace connected to an argon glove box, passing high-purity hydrogen into the closed high-temperature furnace, starting from room temperature, heating at 5-10°C / min to 300-400°C, and keeping it warm for 1-3 hours; turning off the hydrogen and passing high-purity argon, starting from 300-400°C, heating at 5-10°C / min to 500-600°C, and keeping it warm for 1-3 hours, to obtain uranium powder. More preferably, the concentrated nitric acid is 50% concentrated nitric acid by volume. More preferably, the concentrations of water and oxygen in the argon glove box are both lower than 1ppm to avoid the introduction of oxygen to generate oxides. More preferably, the hydrogen and argon heating operations are repeated once or twice. The heating rate, temperature range and insulation time are adjusted to ensure that the metal uranium ingot is completely hydrogenated and dehydrogenated and oxidation is reduced.

[0007] In step S2 of the preferred embodiment, the volume percentage of nitrogen in the mixture of nitrogen and inert gas is 40-50 vol%. More preferably, the inert gas is argon. More preferably, the mixture of nitrogen and inert gas is a mixture of nitrogen and argon mixed in a volume ratio of 1:1. More preferably, the gas is continuously introduced during the heating and cooling process to ensure sufficient nitrogen content. Since more non-stoichiometric uranium nitrogen compounds are easily produced during the nitriding of metal uranium, the length of the insulation time is controlled according to the powder content, and the heating rate, temperature range and insulation time are adjusted to ensure that the metal uranium nitriding reaction is fully carried out, and a pure UN2 first powder is obtained to avoid obtaining other non-stoichiometric uranium nitrogen compound impurities (such as U2N3, etc.). More preferably, a tablet press is used to maintain a pressure of 4-7 tons for 10-20 minutes, and then a pressure of 7-9 tons is maintained for 20-30 minutes, and the first powder is pressed into a first green body with a diameter of 5-20 mm. More preferably, the uranium powder is placed in a heating furnace after grinding, the grinding operation temperature is 10-25°C, and the water and oxygen contents are both less than 0.1ppm. Since the powder particle size is less than 30 microns, the powders are not easy to stick together. The first powder pressing fully discharges the gas between the powders, and ensures sufficient powder pressing time to discharge the gas inside the powder as much as possible, and the spacing between the powders is uniform. The second time, a higher pressure is used to press the powder to make the powder more compact, and the surface layer has the highest compactness, which is convenient for peeling off from the coating layer. The two steps of pressing ensure that the refined powder maintains the complete first green body morphology for subsequent transfer and high temperature experiments.

[0008] Preferably, the high vacuum atmosphere during the sintering process is 5×10 -3 ~5×10 -1Pa; preferably, the protective wrapping layer is resistant to high temperatures and not easy to react with the blank, preferably graphite; at the same time, a protective wrapping layer of a material with high temperature oxygen absorption is added, preferably metal tantalum; and the wrapped blank is placed in a high temperature resistant graphite mold. In step S3 of the preferred embodiment, the first blank is completely wrapped on all sides with tantalum foil and then loaded into a graphite mold, placed in a high temperature furnace, and fired into a porous second blank, and the sintering process is carried out in a vacuum atmosphere. Wrapping on all sides can avoid oxidation reactions. By adjusting the heating rate, temperature range and holding time, it is ensured that the pure UN2 first blank completely separates excess nitrogen in the form of nitrogen gas during the high temperature denitrification reaction to form a pure UN second blank.

[0009] In step S4 of the preferred embodiment, the second green body is surface-cleaned, and the second powder is made by crushing, grinding and sieving. The tablet press is used to maintain a pressure of 4 to 7 tons for 10 to 20 minutes, and then the pressure of 7 to 9 tons is maintained for 20 to 30 minutes, and the second powder is pressed into a third green body with a diameter of 5 to 20 mm. Since the particle size of the powder particles is less than 30 microns, the powders are not easy to stick together. The first pressing of the powder fully discharges the gas between the powders, and ensures that the powder pressing time is sufficient to discharge the internal gas of the powder as much as possible, and the spacing between the powders is uniform. The second time, a higher pressure is used to press the powder to make the powder more compact, and the surface layer has the highest compactness, which is convenient for peeling from the coating layer. Two steps of pressure are applied to ensure that the refined powder maintains the complete first green body morphology for subsequent transfer and high temperature experiments. More preferably, the grinding operation temperature is 10 to 25 ° C, and the water and oxygen contents are both less than 0.1 ppm. More preferably, the specific operation of obtaining the powder of this size is to pass the ground powder through a sieve with 25 μm holes, collect the powder that does not pass through the sieve hole and continue to grind. Repeat the above steps until all the powder passes through the sieve holes and is collected for later use.

[0010] Step S5 uses a fast heating rate and a short holding time and a constant pressure treatment, which, on the one hand, makes the green body quickly densified and crystallized, facilitating the removal of surface impurities, and on the other hand, reduces the time for reaction with trace oxygen and reduces the oxygen content inside the dense core block. Preferably, the high vacuum atmosphere during the sintering process is 5×10 -3 ~5×10 -1 Pa; preferably, the protective wrapping layer is resistant to high temperature and not easy to react with the blank, preferably graphite; at the same time, a protective wrapping layer of a material with high temperature oxygen absorption is added, preferably metal tantalum; and the wrapped blank is placed in a high temperature resistant graphite mold. In step S5 of the preferred embodiment, tantalum foil and 0.1-0.2 mm graphite paper are used to completely wrap the third blank on all sides, and then the third blank is placed in a graphite sintering mold and placed in a high temperature rapid sintering furnace. The sintering process is in a vacuum atmosphere. More preferably, a pre-compression pressure of 10-25 MPa is applied axially to the third blank before heating.

[0011] The uranium nitride nuclear fuel pellet according to the present invention is obtained according to the above-mentioned preparation method.

[0012] According to the preparation method of uranium nitride nuclear fuel pellets of the present invention, uranium blocks are prepared into uranium powder through hydrogenation and dehydrogenation, the uranium powder is ground and placed in a heating furnace into which high-purity nitrogen or a nitrogen and argon mixture is introduced for heating, and cooled in the furnace to form a first powder, and then the first powder is pressed into a first green body, the first green body is placed in a high-temperature heating furnace in a vacuum atmosphere for sintering to obtain a second green body, the second green body is surface-cleaned, and a second powder of micron size is obtained by crushing, grinding and sieving, and then the powder is pressed into a third green body, the third green body is placed in a sintering mold, and the temperature is increased and sintered to obtain a high-density uranium nitride nuclear fuel pellet. The nitride nuclear fuel pellets prepared by the method have the advantages of high density and high radiation stability (no radiation expansion), and can be used as a new type of nuclear fuel for nuclear reactors. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The figures are scanning electron microscope images (SEM) and atomic force microscope detection method (AFM) images of irradiated (Irradiation) and unirradiated (Unirradiation) areas of a fuel pellet prepared according to a preferred embodiment of the present invention.

[0014] Figure 2 1 and 2 are grazing incidence X-ray diffraction (GIXRD) and conventional X-ray diffraction (XRD) images of irradiated (Irradiation) and unirradiated (Unirradiation) regions of a fuel pellet prepared according to an embodiment of the present invention. DETAILED DESCRIPTION

[0015] The preferred embodiments of the present invention are given below in conjunction with the accompanying drawings and described in detail.

[0016] Example 1

[0017] Use 50v% concentrated nitric acid and anhydrous ethanol to clean the surface of the metal uranium block. Polish and polish the surface oxide in the glove box. Put the metal uranium block into a tungsten crucible and place it in a closed high-temperature furnace connected to an argon glove box (water and oxygen <1ppm). Pass high-purity hydrogen into the closed high-temperature furnace, and increase the temperature from room temperature to 300℃ at 5℃ / min, and keep it warm for 2.5h. Turn off the hydrogen and pass high-purity argon, and start from 300℃ and increase the temperature to 500℃ at 5℃ / min, and keep it warm for 2h. Repeat the ventilation and heating operation once.

[0018] The uranium powder is ground and placed in a closed heating furnace of high-purity nitrogen, and the gas is continuously introduced during the heating and cooling process. Specifically, the temperature is raised to 400°C at a rate of 8°C / min, kept at this temperature for 3 hours, and cooled in the furnace to form a first uranium dinitride powder. The first uranium dinitride powder is pressed into a first green body with a diameter of 5 mm using a tablet press at a pressure of 4 tons for 20 minutes and then at a pressure of 7 tons for 25 minutes.

[0019] The first green body is completely wrapped with tantalum foil and then placed in a graphite mold, which is then placed in a high-temperature furnace to be fired into a porous second green body. The sintering process is in a vacuum atmosphere, with the temperature rising to 280°C at a rate of 20°C / min, and then rising to 1450°C at a rate of 10°C / min, and then kept at this temperature for 2 hours, and then cooled with the furnace.

[0020] The second green body is cleaned from the surface, crushed, ground and sifted to form a second powder with a size of 10 to 25 microns, which is then pressed into a third green body; a tablet press is used to press the second powder into a third green body with a diameter of 5 mm at a pressure of 4 tons for 20 minutes and then at a pressure of 7 tons for 25 minutes.

[0021] The third body is completely wrapped with tantalum foil and 0.1mm graphite paper and then placed in a high-temperature rapid sintering furnace to be sintered into a dense fuel pellet. The third body is placed in a graphite sintering mold and the entire sintering process is in a vacuum atmosphere. A pre-compression pressure of 25MPa is applied to the axial direction of the third body before heating. The temperature is raised to 1400℃ at a rate of 90℃ / min, kept warm for 20min, and a constant pressure of 50MPa is applied to the axial direction of the third body. The density of the prepared UN pellet is 9.21g / cm 3 , density is 64.3% TD.

[0022] Example 2

[0023] Use 50v% concentrated nitric acid and anhydrous ethanol to clean the surface of the metal uranium block. Polish and remove the surface oxide in the glove box. Put the metal uranium block into a tungsten crucible and place it in a closed high-temperature furnace connected to an argon glove box (water and oxygen <1ppm). Pass high-purity hydrogen into the closed high-temperature furnace, and increase the temperature from room temperature to 350℃ at 10℃ / min, and keep it warm for 1.5h. Turn off the hydrogen and pass high-purity argon, and start from 350℃ and increase the temperature to 550℃ at 10℃ / min, and keep it warm for 1h. Repeat the ventilation and heating operation twice.

[0024] The metal uranium powder is placed in a closed heating furnace with a nitrogen (argon) mixed gas of 40 vol%, and the gas is continuously introduced during the heating and cooling process. Specifically, the temperature is raised to 500° C. at a rate of 10° C. / min, kept at this temperature for 7 hours, and cooled in the furnace to form a first uranium dinitride powder. A tablet press is used to maintain a pressure of 7 tons for 20 minutes, and then to maintain a pressure of 9 tons for 30 minutes, and the first uranium dinitride powder is pressed into a first green body with a diameter of 20 mm.

[0025] The first green body is completely wrapped with tantalum foil and placed in a high-temperature furnace to be fired into a porous second green body. The sintering process is in a vacuum atmosphere, and the temperature is raised to 350°C at a rate of 25°C / min, and then to 1550°C at a rate of 15°C / min, and kept at this temperature for 1 hour, and then cooled with the furnace.

[0026] The second green body is cleaned from the surface, crushed, ground and sifted to form a second powder with a size of 10 to 25 microns, which is then pressed into a third green body; a tablet press is used to press the second powder into a third green body with a diameter of 20 mm at a pressure of 7 tons for 20 minutes and then at a pressure of 9 tons for 30 minutes.

[0027] The third body is completely wrapped with tantalum foil and 0.2mm graphite paper and then placed in a high-temperature rapid sintering furnace to be sintered into a dense fuel core block. The third body is placed in a graphite sintering mold and the entire sintering process is in a vacuum atmosphere. A pre-compression pressure of 25MPa is applied to the axial direction of the third body before heating. The temperature is raised to 1500℃ at a rate of 100℃ / min, kept warm for 5min, and a constant pressure of 50MPa is applied to the axial direction of the third body. The density of the prepared UN core block is 11.86g / cm 3 , density is 82.9% TD.

[0028] Example 3

[0029] Use 50v% concentrated nitric acid and anhydrous ethanol to clean the surface of the metal uranium block. Polish and remove the surface oxide in the glove box. Put the metal uranium block into a tungsten crucible and place it in a closed high-temperature furnace connected to an argon glove box (water and oxygen <1ppm). Pass high-purity hydrogen into the closed high-temperature furnace, and increase the temperature from room temperature to 350℃ at 10℃ / min, and keep it warm for 1.5h. Turn off the hydrogen and pass high-purity argon, and start from 350℃ and increase the temperature to 550℃ at 10℃ / min, and keep it warm for 1h. Repeat the ventilation and heating operation twice.

[0030] The metal uranium powder is placed in a closed heating furnace with a 50 vol% nitrogen (argon) mixed gas, and the gas is continuously introduced during the heating and cooling process. Specifically, the temperature is raised to 500° C. at a rate of 10° C. / min, kept at this temperature for 7 hours, and cooled in the furnace to form a first uranium dinitride powder. A tablet press is used to maintain a pressure of 7 tons for 15 minutes, and then to maintain a pressure of 9 tons for 20 minutes, and the first uranium dinitride powder is pressed into a first green body with a diameter of 13 mm.

[0031] The first green body is completely wrapped with tantalum foil and placed in a high-temperature furnace to be fired into a porous second green body. The sintering process is in a vacuum atmosphere, and the temperature is raised to 350°C at a rate of 25°C / min, and then to 1550°C at a rate of 15°C / min, and kept at this temperature for 1 hour, and then cooled with the furnace.

[0032] The second green body is cleaned from the surface, crushed, ground and sifted to form a second powder with a size of 10 to 25 microns, which is then pressed into a third green body; a tablet press is used to press the second powder into a third green body with a diameter of 13 mm at a pressure of 7 tons for 15 minutes and then at a pressure of 9 tons for 20 minutes.

[0033] The third body is completely wrapped with tantalum foil and 0.2mm graphite paper and then placed in a high-temperature rapid sintering furnace to be sintered into a dense fuel pellet. The third body is placed in a graphite sintering mold and the entire sintering process is in a vacuum atmosphere. A pre-compression pressure of 10MPa is applied to the axial direction of the third body before heating. The temperature is raised to 1500℃ at a rate of 110℃ / min, kept warm for 20min, and a constant pressure of 30MPa is applied to the axial direction of the third body. The density of the prepared UN pellet is 11.99g / cm 3 , density is 83.7% TD.

[0034] Example 4

[0035] Use 50v% concentrated nitric acid and anhydrous ethanol to clean the surface of the metal uranium block. Polish and remove the surface oxide in the glove box. Put the metal uranium block into a tungsten crucible and place it in a closed high-temperature furnace connected to an argon glove box (water and oxygen <1ppm). Pass high-purity hydrogen into the closed high-temperature furnace, and increase the temperature from room temperature to 350℃ at 10℃ / min, and keep it warm for 1.5h. Turn off the hydrogen and pass high-purity argon, and start from 350℃ and increase the temperature to 550℃ at 10℃ / min, and keep it warm for 1h. Repeat the ventilation and heating operation twice.

[0036] The metal uranium powder is placed in a closed heating furnace with a 50 vol% nitrogen (argon) mixed gas, and the gas is continuously introduced during the heating and cooling process. Specifically, the temperature is raised to 500° C. at a rate of 10° C. / min, kept at this temperature for 7 hours, and cooled in the furnace to form a first uranium dinitride powder. A tablet press is used to maintain a pressure of 7 tons for 15 minutes, and then to maintain a pressure of 9 tons for 20 minutes, and the first uranium dinitride powder is pressed into a first green body with a diameter of 13 mm.

[0037] The first green body is completely wrapped with tantalum foil and placed in a high-temperature furnace to be fired into a porous second green body. The sintering process is in a vacuum atmosphere, and the temperature is raised to 350°C at a rate of 25°C / min, and then to 1550°C at a rate of 15°C / min, and kept at this temperature for 1 hour, and then cooled with the furnace.

[0038] The second green body is cleaned from the surface, crushed, ground and sifted to form a second powder with a size of 10 to 25 microns, which is then pressed into a third green body; a tablet press is used to press the second powder into a third green body with a diameter of 13 mm at a pressure of 7 tons for 15 minutes and then at a pressure of 9 tons for 20 minutes.

[0039] The third body is completely wrapped with tantalum foil and 0.2mm graphite paper and then placed in a high-temperature rapid sintering furnace to be sintered into a dense fuel core block. The third body is placed in a graphite sintering mold. The entire sintering process is in a vacuum atmosphere. A pre-compression pressure of 25MPa is applied to the axial direction of the third body before heating. The temperature is raised to 1600℃ at a rate of 110℃ / min, kept warm for 20min, and a constant pressure of 50MPa is applied to the axial direction of the third body. The density of the prepared UN core block is 13.79g / cm 3 , density is 96.3% TD.

[0040] According to the above example, the irradiation experiment was carried out on the UN sample with the highest density. Figure 2 shown. Figure 1 (a) is a scanning electron microscope image (SEM) of a UN sample irradiated with 1.2 MeV Ar ions at 750 °C. The irradiation dose is 2 × 10 16 ion / cm 2 Since the sample was partially covered by tantalum foil, Figure 1 The left part of (a) is the irradiated area (Irradiation), and the right part is the unirradiated area (Unirradiation), so that the swelling phenomenon before and after irradiation can be clearly observed. The surface roughness of the two areas is tested using atomic force microscopy (AFM), which can accurately determine the surface roughness at the nanoscale, thereby determining the degree of irradiation swelling. Figure 1(b) shows the irradiated and unirradiated boundary images observed by AFM, confirming that the test selected the position with the most significant distinction. Figure 1 (c) is the two-dimensional surface roughness image tested by AFM; Figure 1 (d) is the three-dimensional surface roughness image tested by AFM. The results show that the surface roughness of the UN sample is about 20nm, and the irradiated area does not show a roughness change or height difference beyond this range relative to the non-irradiated area. At the same time, grazing incidence X-ray diffraction (GIXRD) and conventional X-ray diffraction (XRD) were used to test the changes in lattice parameters before and after irradiation, such as Figure 2 As shown in (a) and (b), the spectra of the two samples after irradiation show no difference outside the error range compared with those before irradiation. Based on the above test methods and analysis, it is confirmed that the sample does not show irradiation swelling after irradiation with the irradiation parameters. The UN pellet has high irradiation stability and can be used as a new candidate nuclear fuel for nuclear reactors.

[0041] According to the preparation method of UN fuel of the present invention, high-activity metal uranium powder is used as raw material and no additive sintering agent is used. Therefore, the introduction of impurities is greatly avoided, and the blank does not need to be degreased and dehydrogenated, thereby reducing the heat treatment operation process and the insulation time. The present invention reasonably controls the heating rate, temperature range and insulation time to ensure that each step of the reaction is sufficient and a stable single product is generated, especially the UN2 without impurities generated in the metal uranium nitridation reaction, and the UN powder generated by the UN2 denitrification reaction. The present invention adopts a rapid heating and high-temperature pressure reaction operation, which not only solves the problem of many impurities in the traditional pressureless sintering and hot isostatic pressing sintering products, but also overcomes the shortcomings of long heat treatment time (at least more than ten hours), easy introduction of impurities (such as trace oxygen, carbon) and large product porosity, thereby improving the density and purity of UN fuel, which is conducive to improving the performance of UN fuel. In particular, the nitride nuclear fuel pellets prepared by the present invention have high density, and there is no radiation expansion phenomenon after high-energy Ar ion irradiation, that is, high radiation stability. Therefore, the method can prepare uranium nitride nuclear fuel pellets with high density and good radiation resistance, so that this type of pellets are qualified for use in nuclear reactors and can be used as a new type of nuclear fuel for nuclear reactors.

[0042] The above is only a preferred embodiment of the present invention, and is not intended to limit the scope of the present invention. The above embodiment of the present invention can also be modified in various ways. That is, all simple, equivalent changes and modifications made according to the claims and the description of the present invention fall within the scope of protection of the claims of the present invention. The contents not described in detail in the present invention are all conventional technical contents.

Claims

1. A method for preparing uranium nitride nuclear fuel pellets, characterized in that: The preparation method comprises the following steps: S1, preparing uranium powder from uranium blocks by hydrogenation and dehydrogenation; S2, placing the uranium powder in a heating furnace into which high-purity nitrogen or a mixture of nitrogen and an inert gas is introduced, heating the uranium powder to 300° C. to 600° C. at a rate of 5 to 10° C. / min, maintaining the temperature for 3 to 8 hours, cooling the uranium powder along with the furnace to form a first powder, and then pressing the first powder into a first green body at a pressure of 4 to 9 tons; S3, placing the first green body in a high temperature heating furnace in a vacuum atmosphere, heating the first green body to 250-350° C. at a rate of 10-30° C. / min, then heating the first green body to 1300-1600° C. at a rate of 10-30° C. / min, keeping the temperature for 1-5 hours, and cooling the green body in the furnace to obtain a second green body; S4, forming the second green body into a second powder material having a size of 10 to 25 microns, and then pressing the second powder material into a third green body under a pressure of 4 to 9 tons; S5, placing the third green body in a high-temperature rapid sintering furnace in a vacuum atmosphere, heating the body to 1400-1600° C. at a rate of 90-110° C. / min, keeping the temperature for 5-20 min, applying a constant pressure of 30-50 MPa axially to the third green body, and sintering the body to obtain uranium nitride nuclear fuel pellets.

2. The preparation method according to claim 1, characterized in that: Step S1 comprises: externally using concentrated nitric acid and anhydrous ethanol to clean the surface of the uranium block, grinding and polishing in a glove box to remove the surface oxide, then putting the uranium block into a tungsten crucible, placing it in a closed high-temperature furnace connected to an argon glove box, passing high-purity hydrogen into the closed high-temperature furnace, heating the room temperature to 300-400° C. at a rate of 5-10° C. / min, and keeping the temperature for 1-3 hours; turning off the hydrogen and passing high-purity argon, heating the room temperature to 500-600° C. at a rate of 5-10° C. / min, and keeping the temperature for 1-3 hours to obtain uranium powder.

3. The preparation method according to claim 2, characterized in that: Repeat the heating operation of passing hydrogen and argon once or twice.

4. The preparation method according to claim 1, characterized in that: In step S2, the first powder is pressed into a first green body with a diameter of 5 to 20 mm using a tablet press at a pressure of 4 to 7 tons for 10 to 20 minutes and then at a pressure of 7 to 9 tons for 20 to 30 minutes.

5. The preparation method according to claim 1, characterized in that: In step S3, the first green body is completely wrapped with tantalum foil and then placed in a graphite mold, which is then placed in a high-temperature furnace and sintered into a porous second green body. The sintering process is performed in a vacuum atmosphere.

6. The preparation method according to claim 1, characterized in that: In step S4, the second green body is surface-cleaned, crushed, ground, and sieved to form a second powder, which is then pressed into a third green body having a diameter of 5 to 20 mm using a tablet press at a pressure of 4 to 7 tons for 10 to 20 minutes and then at a pressure of 7 to 9 tons for 20 to 30 minutes.

7. The preparation method according to claim 6, characterized in that: The ground powder is passed through a sieve with 25 μm holes, and the powder that does not pass through the sieve holes is collected and continued to be ground.

8. The preparation method according to claim 1, characterized in that: In step S5, the third green body is completely wrapped with tantalum foil and 0.1-0.2 mm graphite paper, then placed in a graphite sintering mold and placed in a high-temperature rapid sintering furnace. The sintering is performed under a vacuum atmosphere throughout the process.

9. The preparation method according to claim 8, characterized in that: Before heating, a pre-pressing pressure of 10 to 25 MPa is applied axially to the third blank.

10. A uranium nitride nuclear fuel pellet, characterized in that: The uranium nitride nuclear fuel pellet is obtained according to the preparation method described in any one of claims 1-9.

Citation Information

Patent Citations

  • Preparation method of MAX-phase-imitating accident fault-tolerant nuclear fuel pellet

    CN106927832A

  • Method for preparing uranium nitride pellet

    CN108305693A

  • Preparation method of uranium nitride composite uranium dioxide fuel pellet

    CN113012833A

  • Preparation method of uranium nitride composite uranium silicide fuel pellet

    CN113012834A

  • Preparation method of UN pellet for light water reactor

    CN113012836A

Cited By

  • Preparation method of uranium nitride pellet and uranium nitride pellet

    CN120647389A