Preparation method of continuous carbon film grid of transmission electron microscope

The flat carbon film is formed through powder tableting and vacuum coating technology, and combined with the film-floating module and low-angle transfer technology, the problems of complex, high cost and unstable preparation process of ultra-thin carbon film loading in the existing technology are solved, and the problem of instability of ultra-thin carbon film loading network is realized. Efficient, economical and environmentally friendly preparation methods improve the quality and observation accuracy of transmission electron microscope samples.

CN118919386AActive Publication Date: 2024-11-08PEKING UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410958803.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing ultra-thin continuous carbon film transmission electron microscope network-loading preparation methods have problems such as difficulty in defiling, high cost, and easy wrinkle and contamination of the carbon film, resulting in low preparation efficiency and unstable quality.

Method used

Powder tablets are used as medium to form a flat and dense carbon film by vacuum coating and release liquid. Combined with film scattering modules and low angle transfer technology, the preparation process is simplified and the cost is reduced, and the carbon film is avoided.

Benefits of technology

It improves preparation efficiency, reduces costs, enhances the quality stability and observation accuracy of carbon films, is suitable for substrates of different materials and sizes, and conforms to the principle of green chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919386A_ABST
    Figure CN118919386A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a continuous carbon film grid of a transmission electron microscope, which comprises the following steps: firstly, preparing a low-price medium to form a flat and compact sheet, and plating a continuous carbon film on the medium; the medium covered with the continuous carbon film is clamped by a clamping tool, the other end of the medium makes contact with the liquid level, and the continuous carbon film is released to the liquid level at a certain angle at a constant speed; a carrying net, a substrate and filter paper needing film fishing are placed from top to bottom to form a film fishing module; firstly, the film fishing module enters water at a preset angle, after the film fishing module gets close to the carbon film, the center of the carrier net is aligned with the center of the carbon film, and the carbon film falls onto the carrier net at a constant speed from bottom to top according to the angle smaller than 5 degrees. The air-dried grid can be subjected to annealing and other treatments. By simplifying the preparation process, reducing the cost and improving the quality stability, an efficient, economical and practical solution is provided for sample preparation of the transmission electron microscope, and the method is expected to be widely applied in practical application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a method for preparing a continuous carbon film grid for a transmission electron microscope, belonging to the technical field of transmission electron microscopes. Background Art

[0002] The preparation of ultra-thin continuous carbon film support membrane has important background significance and application value in transmission electron microscopy sample preparation. By in-depth research on the preparation method and optimization of process parameters, the quality and stability of the carbon film can be improved, and simple and effective preparation methods can be explored to provide more reliable tools and means for research in related fields.

[0003] The existing method for preparing ultra-thin continuous carbon film transmission electron microscope grid uses mica as the substrate, which is difficult to remove the film and it is difficult to maintain the integrity of the film. The mica sheet is disposable, resulting in high experimental costs. In addition, the existing method directly uses the grid to scoop up the film, which easily causes carbon film wrinkles and excess carbon film is easily adsorbed to the back of the grid to cause pollution. Therefore, a new preparation method is needed to improve preparation efficiency, reduce costs, and improve quality stability. Summary of the invention

[0004] The present invention aims to provide a method for preparing an ultra-thin continuous carbon film transmission electron microscope grid, which provides an efficient, economical and practical solution for transmission electron microscope sample preparation by simplifying the preparation process, reducing costs and improving quality stability, and can improve the preparation efficiency and observation quality of transmission electron microscope samples.

[0005] The present invention provides a method for preparing an ultra-thin continuous carbon film transmission electron microscope grid, the method comprising the following steps:

[0006] Step 1: Prepare the medium for coating:

[0007] First, prepare a low-cost medium, and use powder tableting as the medium; the medium can form a flat and dense thin sheet. The medium preparation process described in the present invention mainly involves pressing the uncontaminated sample into a flat and dense thin sheet by tableting. The sample is: NaCl, KCl, CaCO 3 、Al 2 O 3 ,BaSO 4 、ZnO、SiO 2 One of the above.

[0008] Step 2: Vacuum coating:

[0009] The continuous carbon film is plated on the medium whose surface can be flat and dense after being pressed by magnetron sputtering, electron beam deposition or carbon evaporation.

[0010] Step 3: Release the carbon film:

[0011] Prepare the release liquid in a certain container, then use a clamping tool to clamp the medium covered with the continuous carbon film, contact the other end of the medium with the liquid surface and release the continuous carbon film onto the liquid surface at a certain angle and at a uniform speed.

[0012] The container described in the present invention is any utensil that can hold solvents, such as a culture dish or a beaker. The release liquid can be non-toxic and low-cost solvents, such as ultrapure water and ethanol. The clamping tool can be a tool with clamping function, such as pointed tweezers and duckbill tweezers.

[0013] Step 4: Build the membrane scooping module:

[0014] Cut filter paper slightly larger than the carrier mesh and a flat and dense substrate with low surface tension (such as glass or silicon wafer, etc.), place the carrier mesh, substrate, and filter paper to be scooped up from top to bottom to form a film scooping module, and fix it with a clamping tool.

[0015] Step 5: Transfer to the carrier network:

[0016] First, place the film scooping module into the water at a certain angle, align the center of the carrier grid and the carbon film when it is close to the carbon film, and drop the carbon film onto the carrier grid at a constant speed from bottom to top at an angle less than 5°.

[0017] Step 6: Post-processing:

[0018] Place the membrane module gently on the filter paper and wait for it to dry naturally. The dried carrier grid can be annealed to optimize the structure and performance of the carbon membrane and improve its stability and applicability.

[0019] Step 7: Testing and Evaluation:

[0020] The prepared ultra-thin continuous carbon film is tested and evaluated, and can be used if it meets the requirements.

[0021] Through the above method, the present invention achieves the following advantages:

[0022] Simplify the preparation process: By adopting a simple and effective preparation method, the complexity of the preparation process is reduced and the preparation efficiency is improved;

[0023] Reduce costs: Use low-cost raw materials and equipment to reduce preparation costs, making large-scale production possible;

[0024] Improve quality stability: By optimizing the preparation process parameters, the quality stability of ultra-thin continuous carbon film is improved, ensuring the accuracy of transmission electron microscopy observation;

[0025] Strong applicability: The method of the present invention is applicable to substrates of different materials and sizes and has a wide range of applications;

[0026] Environmentally friendly and non-toxic: The materials used in the preparation process are environmentally friendly and non-toxic, in line with the principles of green chemistry.

[0027] In summary, the present invention provides a method for preparing an ultra-thin continuous carbon film transmission electron microscope grid, aiming to solve the problems of complex transmission electron microscope grid preparation process, high cost and unstable quality in the prior art. By simplifying the preparation process, reducing costs and improving quality stability, an efficient, economical and practical solution is provided for transmission electron microscope sample preparation, which is expected to be widely used in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart of preparing an ultra-thin continuous carbon film grid;

[0029] Figure 2a This is one of the transmission electron microscope characterization images of the ultra-thin continuous carbon film grid of the embodiment;

[0030] Figure 2b The second transmission electron microscope characterization image of the ultra-thin continuous carbon film grid of the embodiment;

[0031] Figure 2c The third transmission electron microscope characterization image of the ultra-thin continuous carbon film grid of the embodiment;

[0032] Figure 3a One of the TEM images of the statistical carbon film coverage and contamination rate of the embodiment;

[0033] Figure 3b The second TEM image of the statistical carbon film coverage and contamination rate of the embodiment;

[0034] Figure 3c The third TEM image of the statistical carbon film coverage and contamination rate of the embodiment;

[0035] Figure 3d The fourth TEM image of the statistical carbon film coverage and contamination rate of the embodiment;

[0036] Figure 4a This is one of the TEM images of the embodiment under high magnification characterizing the continuous carbon film in the pores;

[0037] Figure 4b This is the second TEM image of the embodiment characterizing the continuous carbon film in the pores at high magnification;

[0038] Figure 5a One of the transmission electron microscope images of a 2nm ultra-thin continuous carbon film copper mesh prepared in Example;

[0039] Figure 5b The second transmission electron microscope image of a 2nm ultra-thin continuous carbon film copper mesh prepared in Example;

[0040] Figure 5cThe third transmission electron microscope image of a 2nm ultra-thin continuous carbon film copper mesh prepared in Example;

[0041] Figure 6a This is one of the cryo-electron microscopy characterization images of a human ferritin sample prepared by laying a 2 nm continuous carbon film grid in the example;

[0042] Figure 6b This is the second cryo-electron microscopy characterization image of the human ferritin sample prepared using a 2 nm continuous carbon film grid in the example. DETAILED DESCRIPTION

[0043] like Figure 1 The process shown includes the following steps:

[0044] The first step is to prepare the coating medium: first prepare a low-cost NaCl sample, apply a pressure of 10Mpa through a tablet press, and press the NaCl sample into a 5mm diameter tablet.

[0045] The second step is vacuum coating: Place the 5mm diameter wafer into the vacuum coating equipment. After the vacuum value reaches 2×10-6mbar, control the coating parameters and use electron beam deposition to deposit a 2nm thick carbon film on the NaCl medium.

[0046] Step 3: Release the carbon film: prepare a petri dish and add deionized water to it. Then use tweezers to clamp one end of the NaCl medium coated with a 2nm carbon film, and contact the liquid surface with the other end at an angle of about 30°, and release the continuous carbon film to float on the water surface at a uniform speed.

[0047] Step 4: Build the membrane scooping module: cut filter paper of about 5 mm, cut a glass slide of about 5 mm, prepare a clean 3 mm grid, and use tweezers to clamp the grid, glass slide, and filter paper from top to bottom at the same time.

[0048] The membrane blocks can be replaced by a container with a controllable flow rate, which can play the same role.

[0049] Step 5: Transfer to the grid: First, place the film scooping module into the water at a certain angle, align the center of the grid and the carbon film when it is close to the carbon film, and drop the carbon film onto the grid at a constant speed from bottom to top at an angle less than 5°.

[0050] Step 6: Post-processing: Gently place the membrane module on the filter paper and wait for it to air dry for 15 minutes. The air-dried grid can be heated and annealed at 150℃ for 1 hour.

[0051] Step 7, testing and evaluation: The prepared ultra-thin continuous carbon film can be tested and evaluated under an optical microscope. If the coverage is higher than 80%, the breakage rate is lower than 10%, and the contamination rate is lower than 10%, it can be used if it meets the requirements.

[0052] like Figure 2a to Figure 2c The figure shows different magnifications of a 2nm continuous carbon film prepared by using a 400-mesh array gold grid, and the pictures were taken by a Talos L120CG2 transmission electron microscope. The results show that the 2nm ultra-thin continuous carbon film grid prepared by the present invention is very clean as a whole, and the carbon film is very flat.

[0053] like Figure 3a to Figure 3d The figure shows the pictures taken by transmission electron microscope at different positions randomly selected in the same carrier grid, where the rectangle represents the seriously contaminated holes and the circle represents the broken holes. The statistical results show that there are 900 holes in 4 arrays, 9 of which are contaminated, that is, the contamination rate is 1%, and 5 of which are broken, that is, the coverage rate is as high as 99.4%. The statistical results confirm that the coverage rate of ultra-thin carbon film can be greatly improved by the experimental method of the present invention.

[0054] like Figure 4a and Figure 4b As shown, the high-magnification photograph of the carbon film in the pores taken at 12000 times with a 120kV transmission electron microscope clearly shows the smooth carbon film, and the Fourier ring strongly proves that the carbon film prepared by the present invention is a continuous, smooth and high-quality carbon film.

[0055] like Figure 5a to Figure 5c As shown in FIG. 1 , the results of characterization using a 120 kV transmission electron microscope using a grid of another specification are shown. The grid used is a 300-mesh copper grid and the carbon film thickness is 2 nm. The results show that for this type of grid, a complete, continuous, and high-quality carbon film can still be obtained using the method of the present invention.

[0056] like Figure 6a and Figure 6b As shown in the figure, a 0.5 mg / mL human ferritin sample was frozen and characterized by a 200kVTalos Arctica field emission cryo-electron microscope. The results show that laying a continuous carbon film can greatly improve the sample concentration, and it can also prove that the continuous carbon film in the pores is continuous and flat. Figure 6b The CTF shown is at higher resolution.

[0057] The substrate of the present invention is different from the traditional single crystal NaCl: the substrate of the present method is easy to prepare, cheap, is a water-soluble powder (particle size 1.0 μm-100.0 μm), is easy to demould, flat, and has good integrity;

[0058] Compared with mica sheets, the substrate of the present invention is easy to prepare, cheap, and is a water-soluble powder (particle size 1.0 μm-100.0 μm), easy to demould, and has high demould integrity;

[0059] Compared with the film scooping method of directly scooping the film from bottom to top using a carrier mesh: this method builds a film scooping module, avoids the problems of carbon film breakage, undulation and excess carbon film being easily adsorbed to the back of the carrier mesh and causing pollution due to excessive surface tension when the carbon film is directly scooped using a carrier mesh, and can greatly improve the flatness, integrity and coverage of the film scooping.

Claims

1. A method for preparing a continuous carbon film grid for transmission electron microscopy, characterized in that: The following steps are involved: The first step is to prepare the coating medium; First, the medium is prepared, and the medium forms a flat and dense sheet; The second step is vacuum coating; Coating a continuous carbon film on a flat medium; Step 3: Release the carbon film; Prepare a release liquid in a container, then clamp the medium covered with the continuous carbon film with a clamping tool, contact the other end of the medium with the liquid surface and release the continuous carbon film onto the liquid surface at a constant speed according to a preset angle; Step 4: Build the membrane scooping module; Cut filter paper larger than the carrier mesh and a flat and dense substrate with low surface tension, place the carrier mesh that needs to be scooped up from top to bottom, and the substrate and filter paper form a scooping module, which is fixed with a clamping tool; Step 5: Transfer to the carrier network; Then, the carbon film is dropped completely onto the film scooping module from bottom to top at a preset angle; Step 6: Post-processing; Place the membrane module gently on the filter paper and wait for it to dry naturally; perform post-processing on the dried carrier mesh; Step 7: Testing and evaluation; The prepared ultra-thin continuous carbon film is tested and evaluated, and can be used if it meets the requirements.

2. The method for preparing a continuous carbon film grid for transmission electron microscopy according to claim 1, characterized in that: In the first step, powder tablets are used as the medium, and the powder material is one of NaCl, KCl, CaCO3, Al2O3, BaSO4, ZnO, SiO2, etc.

3. The method for preparing a continuous carbon film grid for transmission electron microscopy according to claim 1, characterized in that: In the second step, vacuum coating is performed by magnetron sputtering, electron beam deposition or carbon evaporation.

4. The method for preparing a continuous carbon film grid for transmission electron microscopy according to claim 1, characterized in that: In the third step, the release liquid is ultrapure water or ethanol.

5. The method for preparing a continuous carbon film grid for transmission electron microscopy according to claim 1, characterized in that: The substrate in the fourth step is a glass wafer or a silicon wafer.

6. The method for preparing a continuous carbon film grid for transmission electron microscopy according to claim 1, characterized in that: The sixth step is post-processing, including annealing.

Citation Information

Patent Citations

  • Preparation method for carbon extraction replica sample of transmission electron microscope

    CN103344466A

  • Improved preparation of cryogenic sample, e.g. for charged particle microscopy

    CN109900729A

  • Oxidized graphene carbon support film transmission electron microscope (TEM) grid

    CN109950117A

  • Preparation method of microarray ultrathin support film for transmission electron microscope analysis

    CN110702703A

  • Preparation method of electron microscope array carrier net

    CN111370279A