Epitaxial wafer structure and preparation method thereof

By using composite substrate with Si/insulating material/SiO2 or Si/insulating material/Si3N4 structure in the nitride epitaxial sheet and oxidation or nitriding process, the insulating dielectric layer is formed, and the breakdown of the nitride epitaxial sheet at high voltage is solved. and stress control problems improve the device's voltage withstand uniformity and reduce production costs.

CN118919399APending Publication Date: 2024-11-08NINGBO GRAPHENE INNOVATION CENT CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411000308.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Nitride epitaxial sheets are prone to breakdown at high voltages, and stress and warping are difficult to control when growing thick films, which affects the uniformity and voltage resistance of the device and increases production costs.

Method used

A composite substrate with Si/insulating material/SiO2 or Si/insulating material/Si3N4 structure is used, and an insulating dielectric layer, growth buffer layer and barrier layer are formed through oxidation or nitriding processes to reduce the silicon substrate and nitride epitaxial layer. Interface stress improves the pressure resistance and uniformity of the epitaxial sheet.

Benefits of technology

Effectively improve the pressure resistance of nitride epitaxial sheets, reduce growth time and cost, and improve the yield of epitaxial sheets and chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919399A_ABST
    Figure CN118919399A_ABST
Patent Text Reader

Abstract

The invention discloses an epitaxial wafer structure and a preparation method thereof. The epitaxial wafer structure comprises a Si / insulating material / Si structure composite substrate, a transition layer, a buffer layer on the transition layer, a channel layer above the buffer layer, and a barrier layer above the channel layer. And after the transition layer is grown, oxidizing or nitriding the silicon material layer between the transition layer and the insulating material in the substrate through an oxidizing or nitriding process to form a silicon dioxide or silicon nitride insulating dielectric layer. And sequentially growing a buffer layer, a channel layer and a barrier layer above the transition layer according to a common nitride epitaxial growth process. The voltage resistance of the nitride epitaxial wafer can be effectively improved by converting the silicon material between the insulating materials in the epitaxial layer and the substrate into the insulating silicon dioxide or silicon nitride material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductors, and in particular relates to an epitaxial wafer structure and a preparation method thereof. Background Art

[0002] As a new type of wide bandgap semiconductor, nitride power devices have high breakdown electric field, more energy saving, more stable physical and chemical properties, can work at higher ambient temperature, have higher switching speed, can reduce the volume and weight of application systems, and other advantages compared with traditional silicon devices. They can be applied to various household appliances, electric vehicles, solar and wind energy and other new energy generation, electric vehicles, robots, intelligent manufacturing industry, large data processing centers and other fields. However, nitride power devices are currently mainly used in the field of medium and low voltage consumer electronics. One of the reasons is that nitride epitaxial materials use heteroepitaxial methods to grow nitride semiconductor thin film materials on large-sized silicon substrates. Because a conductive channel is formed at the interface between the silicon substrate and the nitride epitaxial layer, the device tends to break down first in the vertical direction under high voltage, and the withstand voltage of gallium nitride power devices is limited by the withstand voltage of the epitaxial material in the vertical direction. Increasing the thickness of the epitaxial material can improve the material's withstand voltage accordingly, but due to the mismatch between the silicon substrate and the nitride epitaxial material in terms of lattice size and thermal expansion coefficient, the thicker the epitaxial layer is grown, the greater the stress inside the epitaxial wafer, making it difficult to control the stress and warping of the epitaxial wafer. At the same time, since the warping of the epitaxial wafer also increases accordingly during the growth of the thick film, the growth conditions at different positions of the epitaxial wafer will have greater differences, reducing the uniformity of various parameters of the epitaxial wafer. The warping control problem and the uniformity problem of the epitaxial wafer will affect the yield and cost of the final product. In addition, the thicker the epitaxial material is grown, the longer the growth time required will be. Since epitaxial production equipment is very expensive, this will also increase the cost of the product. Summary of the invention

[0003] In response to the problems in the background technology, the present invention provides an epitaxial wafer structure, including: a composite substrate, a transition layer, a buffer layer on the transition layer, a channel layer above the buffer layer, and a barrier layer above the channel layer, wherein the composite substrate is a Si / insulating material / SiO2 structure or a Si / insulating material / Si3N4 structure.

[0004] The present invention also provides a method for preparing an epitaxial wafer, which is at least used to prepare the above-mentioned epitaxial structure, comprising the following steps:

[0005] S1. Providing a Si / insulating material / Si structure substrate and growing a transition layer on the substrate;

[0006] S2, oxidizing or nitriding the silicon material layer between the transition layer and the insulating material in the substrate through an oxidation or nitridation process to form a silicon dioxide or silicon nitride insulating dielectric layer;

[0007] S3. A buffer layer, a channel layer and a barrier layer are grown in sequence on the transition layer according to a common nitride epitaxial growth process.

[0008] Optionally, Si / insulating material / Si is a Si / SiO2 / Si structure or a Si / AlN / Si structure, or other Si / insulating material / Si structures.

[0009] Optionally, the transition layer is selected from one of the following materials: gallium nitride, aluminum nitride, indium nitride, or alloy materials or multi-layer stacked structures of the above materials; or 3C-SiC material, SiN material; or first growing a layer of 3C-SiC or SiN material on the surface of the silicon substrate, and then continuing to grow the above-mentioned gallium nitride, aluminum nitride, indium nitride, or alloy materials of the above materials or a multi-layer stacked structure of the above materials.

[0010] Optionally, the oxidation process is selected from one of the following processes: dry oxidation process, wet oxidation process, oxygen ion implantation process. The dry oxidation process uses oxygen or oxide-containing gas to react with silicon at high temperature to produce SiO2, and the reaction temperature can be 600-1400°C. The wet oxidation process uses wet oxygen or wet oxide gas to react with silicon at high temperature to produce SiO2, and the reaction temperature can be 600-1400°C. Or, other oxidizing gases such as O3, NO, NO2, SO2 are used to oxidize silicon at high temperature to produce SiO2. Or, the substrate is exposed to a plasma atmosphere containing oxygen elements to oxidize the silicon material at the interface between the nitride and the silicon substrate and convert it into SiO2.

[0011] Optionally, the nitridation process may be performed by nitrogen ion implantation, or by treating the substrate with nitrogen-containing gases such as NH3, NO, etc. at high temperature, or by exposing the substrate to a plasma atmosphere containing the N element, so that the silicon material at the interface between the nitride and the silicon substrate is nitrided and converted into SiN.

[0012] Optionally, the buffer layer is made of one of the following materials: AlN, AlGaN, a GaN single layer or multi-layer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN super lattice structure, or a combination of the above structures.

[0013] Optionally, the channel layer is selected from one of the following materials: GaN material, AlGaN material, and InGaN material.

[0014] Optionally, the barrier layer is selected from one of the following materials: an AlGaN layer, an AlN layer, an AlInN layer, an AlInGaN layer, or a plurality of superpositions of the above material layers.

[0015] Optionally, an AlN insertion layer may be included between the channel layer and the barrier layer.

[0016] Optionally, the barrier layer includes an unintentionally doped GaN cap layer or an in-situ SiN dielectric layer, or an alloy layer of p-type AlGaInN in any proportion.

[0017] Compared with the prior art, the present invention provides an epitaxial wafer structure and a preparation method thereof, which has the following beneficial effects:

[0018] The present invention adopts a Si / insulating material / Si structure composite substrate and converts the silicon material between the epitaxial layer and the insulating material in the substrate into insulating silicon dioxide or silicon nitride material, thereby effectively improving the withstand voltage of the nitride epitaxial wafer, reducing the requirement for the thickness of the epitaxial layer, thereby reducing the difficulty of the growth technology, and can simultaneously reduce the epitaxial growth time, improve the uniformity of epitaxial parameters, thereby improving the yield of the epitaxial wafer and the chip. At the same time, by reducing the thickness of the silicon material on the silicon substrate, the volume expansion of SiO2 formed after dry or wet oxidation and the time required for the dry or wet oxidation process are reduced, or the ion implantation energy and process time required in the ion implantation process are reduced, thereby reducing the process damage to the transition layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of the epitaxial wafer structure of Example 1 of the present invention.

[0020] Figure 2a to Figure 2d This is a flow chart for epitaxial wafer production in Example 1.

[0021] Figure 3 This is a schematic diagram of the epitaxial wafer structure of Example 2 of the present invention.

[0022] Figures 4a to 4d This is a flow chart for epitaxial wafer production in Example 2.

[0023] Figure 5 This is a schematic diagram of the epitaxial wafer structure of Example 3 of the present invention.

[0024] Figures 6a to 6d This is the flow chart for epitaxial wafer production in Example 3.

[0025] Wherein: 10-composite substrate; 101-lower silicon material layer; 102-middle insulating material layer; 103-upper silicon material layer; 103'-insulating dielectric layer (SiO2); 12-transition layer; 13-buffer layer; 14-channel layer; 15-barrier layer 15; 20-composite substrate 20; 201-lower silicon material layer; 202-middle insulating material layer; 203-upper silicon material layer; 203'-insulating dielectric layer 1-SiO2 layer; 22-transition layer; 23-buffer layer; 24-channel layer; 25-barrier layer; 26-p-type GaN layer; 30-composite substrate; 301-lower silicon material layer; 302-middle insulating material layer; 303-upper silicon material layer; 303'-insulating dielectric layer (SiO2); 32-transition layer; 33-buffer layer; 34-channel layer; 35-barrier layer; 36-in-situ SiN layer. DETAILED DESCRIPTION

[0026] The present disclosure will now be described more fully below with reference to the accompanying drawings, however, the present disclosure can be implemented in many different ways and should not be construed as being limited to the embodiments set forth herein. On the contrary, providing these embodiments herein will make the present disclosure more detailed and complete, and fully convey the scope of the present disclosure to those skilled in the art. The same reference numerals throughout the text represent the same objects.

[0027] Example 1

[0028] In the first exemplary embodiment, referring to Figure 1 The structure of the silicon substrate nitride semiconductor epitaxial wafer provided in this embodiment includes a composite substrate 10, and a transition layer 12, a buffer layer 13, a channel layer 14, and a barrier layer 15 formed sequentially on the substrate 10. The composite substrate 10 includes a lower silicon material layer 101, an intermediate insulating material layer 102, and an upper silicon material layer 103. Through a dry oxidation process, the upper silicon material layer 103 between the insulating material layer 102 and the transition layer 12 is transformed into an insulating dielectric layer (SiO2) 103', so that the total thickness of the insulating layer on the surface of the substrate becomes the sum of the thickness of the insulating material layer 102 and the insulating dielectric layer (SiO2) 103'. By providing an additional insulating layer thickness on the basis of the thickness of the nitride epitaxial layer, the voltage resistance of the entire epitaxial wafer can be greatly improved.

[0029] In an optional embodiment, the substrate 10 is a silicon composite substrate, including a lower silicon material layer 101 with a thickness of 670 microns, an intermediate insulating material layer 102 is a SiO2 layer with a thickness of 2 microns, and an upper silicon material layer 103 with a thickness of 1 micron. However, the embodiments of the present disclosure are not limited thereto, and the intermediate insulating material layer may also be a Si / AlN / Si structure, or other Si / insulating material / Si structures; the thickness of the upper silicon material layer, the intermediate insulating material layer, and the lower silicon material layer is between 1 nanometer and 50 microns.

[0030] In an optional embodiment, the transition layer 12 is an AlN layer with a thickness of 0.1-200 nm. However, the embodiments of the present disclosure are not limited thereto, and the transition layer 12 may also be gallium nitride, indium nitride, or their alloy materials or a multilayer stacked structure of the above materials; it may also be a layer of 3C-SiC material or a layer of SiN material; it may also be a layer of 3C-SiC or SiN material grown on the surface of the silicon substrate first, and then the above gallium nitride, aluminum nitride, indium nitride, or their alloy materials or a multilayer stacked structure of the above materials are continued to grow.

[0031] In an optional embodiment, the buffer layer 13 is AlN with a thickness of 0.5-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 13 may also be AlGaN, a GaN single layer or multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.

[0032] In an optional embodiment, the channel layer 14 is made of GaN material with a thickness of 20-1000 nm. However, the embodiments of the present disclosure are not limited thereto, and the channel layer 14 may also be made of AlGaN or InGaN material.

[0033] In an optional embodiment, the barrier layer 15 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer 15 may also be an AlN layer, AlInN, AlInGaN, or a plurality of superpositions of the above material layers.

[0034] In an optional embodiment, an AlN insertion layer is further included below the barrier layer 15 , with a thickness of 0.1-2 nm.

[0035] In an optional embodiment, the barrier layer 15 may include a GaN cap layer with a thickness of 0.1-10 nm, or an in-situ SiN dielectric layer with a thickness of 0.5-150 nm, or a p-type GaN layer with a thickness of 10-200 nm.

[0036] Reference Figure 2a-2d As shown, this embodiment provides a process flow for preparing the nitride semiconductor epitaxial wafer.

[0037] Step 1, such as Figure 2a As shown, a silicon substrate 10 is provided, including a lower silicon material layer 101 with a thickness of 670 microns, an intermediate insulating material layer 102 which is a SiO2 layer with a thickness of 2 microns, and an upper silicon material layer 103 with a thickness of 1 micron.

[0038] Step 2, such as Figure 2bAs shown, a transition layer 12 is grown on the substrate. The growth process is metal organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE), or sputtering, or other vapor deposition processes. In this embodiment, the transition layer is an AlN nucleation layer with a thickness of 100 nm.

[0039] Step 3, such as Figure 2c As shown, the epitaxial wafer after the transition layer 12 is grown is subjected to a dry oxidation process commonly used in silicon processing technology, oxygen is introduced at high temperature, and the upper silicon material layer 103 between the insulating material layer 102 and the transition layer 12 is transformed into an insulating dielectric layer (SiO2) 103'.

[0040] Step 4, such as Figure 2d As shown, after the insulating dielectric layer (SiO2) 103' is grown, a nitride buffer layer is grown on the epitaxial wafer, including a 100nm AlN layer, a 50nm AlGaN layer, and a 3000nm AlN / GaN superlattice structure. A 300nm GaN channel layer, a 1nm AlN insertion layer (not shown in the schematic diagram), and a 25nm AlGaN barrier layer are grown on the buffer layer.

[0041] Example 2

[0042] In the second exemplary embodiment, referring to Figure 1 The structure of the silicon substrate nitride semiconductor epitaxial wafer provided in this embodiment includes a composite substrate 20, and a transition layer 22, a buffer layer 23, a channel layer 24, a barrier layer 25, and a p-type GaN layer 26 formed sequentially on the substrate 20. The composite substrate 20 includes a lower silicon material layer 201, an intermediate insulating material layer 202, and an upper silicon material layer 203. Through a dry oxidation process, the upper silicon material layer 203 between the insulating material layer 202 and the transition layer 22 is transformed into an insulating dielectric layer (SiO2) 203', so that the total thickness of the insulating layer on the surface of the substrate becomes the sum of the thickness of the insulating material layer 202 and the insulating dielectric layer (SiO2) 203'. By providing an additional insulating layer thickness on the basis of the thickness of the nitride epitaxial layer, the withstand voltage of the entire epitaxial wafer can be greatly improved. By changing the SiO2 intermediate layer in the composite substrate to an AlN layer, the thermal conductivity of the substrate can be improved, and by reducing the thickness of the upper silicon material layer 203, the energy of the oxygen ion implantation process can be reduced, and the process damage to the transition layer 22 can be reduced.

[0043] In an optional embodiment, the substrate 20 is a silicon composite substrate, including a lower silicon material layer 201 with a thickness of 670 microns, an intermediate insulating material layer 102 is an AlN layer with a thickness of 5 microns, and an upper silicon material layer 203 with a thickness of 1 micron. However, the embodiments of the present disclosure are not limited thereto, and the thickness of the upper silicon material layer, the intermediate insulating material layer, and the lower silicon material layer is between 1 nanometer and 50 microns.

[0044] In an optional embodiment, the transition layer 22 is an AlN layer with a thickness of 0.1-200 nm. However, the embodiments of the present disclosure are not limited thereto, and the transition layer 22 may also be gallium nitride, indium nitride, or their alloy materials or a multilayer stacked structure of the above materials; it may also be a layer of 3C-SiC material or a layer of SiN material; it may also be a layer of 3C-SiC or SiN material grown on the surface of the silicon substrate first, and then the above gallium nitride, aluminum nitride, indium nitride, or their alloy materials or a multilayer stacked structure of the above materials are continued to grow.

[0045] In an optional embodiment, the buffer layer 23 may include AlN, and the thickness is generally 0.5-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 23 may also be AlGaN, a GaN single layer or multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.

[0046] In an optional embodiment, the channel layer 24 is made of GaN material with a thickness of 20-1000 nm. However, the embodiments of the present disclosure are not limited thereto, and the channel layer 24 may also be made of AlGaN or InGaN material.

[0047] In an optional embodiment, the barrier layer 25 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer 25 may also be an AlN layer, AlInN, AlInGaN, or a plurality of superpositions of the above material layers.

[0048] In an optional embodiment, an AlN insertion layer is further included below the barrier layer, with a thickness of 0.1-2 nm.

[0049] In an optional embodiment, the barrier layer further includes a GaN cap layer with a thickness of 0.1-10 nm, or an in-situ SiN dielectric layer with a thickness of 0.5-150 nm, or a p-type GaN layer with a thickness of 10-200 nm.

[0050] Reference Figure 4a-4d As shown, this embodiment provides a process flow for preparing the nitride semiconductor epitaxial wafer.

[0051] Step 1, such as Figure 4a As shown, a composite substrate 20 is provided, including a lower silicon material layer 201 with a thickness of 670 microns, an intermediate insulating material layer 102 which is an AlN layer with a thickness of 5 microns, and an upper silicon material layer 203 with a thickness of 1 micron.

[0052] Step 2, such as Figure 4bAs shown, a transition layer 22 is grown on the substrate. The growth process is metal organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE), or sputtering process, or other vapor deposition process. The transition layer of this embodiment includes an AlN nucleation layer grown by MOCVD process, and the thickness is 100nm.

[0053] Step 3, such as Figure 4c As shown, the epitaxial wafer after the transition layer 22 is grown is subjected to an oxygen ion implantation process to transform the upper silicon material layer 203 between the insulating material layer AlN 202 and the transition layer 22 into an insulating dielectric layer (SiO2) 203'.

[0054] Step 4, such as Figure 4d As shown, after the insulating dielectric layer (SiO2) 203' is grown, a nitride buffer layer is grown on the epitaxial wafer, including a 100nm AlN layer, a 50nm AlGaN layer, and a 3000nm AlN / GaN superlattice structure. A 300nm GaN channel layer, a 1nm AlN insertion layer (not shown in the schematic diagram), a 25nm AlGaN barrier layer, and an 80nm p-type GaN layer are grown on the buffer layer.

[0055] Example 3

[0056] In the third exemplary embodiment, referring to Figure 5 The structure of the silicon substrate nitride semiconductor epitaxial wafer provided in this embodiment includes a composite substrate 30, and a transition layer 32, a buffer layer 33, a channel layer 34, a barrier layer 35, and an in-situ SiN layer 36 formed sequentially on the substrate 30. The composite substrate 30 includes a lower silicon material layer 301, an intermediate insulating material layer 302, and an upper silicon material layer 303. Through a wet oxidation process, the upper silicon material layer 303 between the insulating material layer 302 and the transition layer 32 is transformed into an insulating dielectric layer (SiO2) 303', so that the total thickness of the insulating layer on the surface of the substrate becomes the sum of the thickness of the insulating material layer 302 and the insulating dielectric layer (SiO2) 303'. By providing an additional insulating layer thickness on the basis of the thickness of the nitride epitaxial layer, the voltage resistance of the entire epitaxial wafer can be greatly improved.

[0057] In an optional embodiment, the substrate 30 is a silicon composite substrate, including a lower silicon material layer 301 with a thickness of 670 microns, an intermediate insulating material layer 302 is an AlN layer with a thickness of 5 microns, and an upper silicon material layer 303 with a thickness of 1 micron. However, the embodiments of the present disclosure are not limited thereto, and the intermediate insulating material layer can also be other insulating materials, and the thickness of the upper silicon material layer, the intermediate insulating material layer, and the lower silicon material layer is between 1 nanometer and 50 microns.

[0058] In an optional embodiment, the transition layer 32 is a 3C-SiC layer with a thickness of 0.1-200 nm. However, the embodiments of the present disclosure are not limited thereto, and the transition layer 32 may also be gallium nitride, aluminum nitride, indium nitride, or their alloy materials or a multilayer stacked structure of the above materials; it may also be a layer of SiN material; it may also be a layer of 3C-SiC or SiN material grown on the surface of the silicon substrate first, and then the above gallium nitride, aluminum nitride, indium nitride, or their alloy materials or a multilayer stacked structure of the above materials are continued to grow.

[0059] In an optional embodiment, the buffer layer 33 is AlN with a thickness of 0.5-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 33 may also be AlGaN, a GaN single layer or multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.

[0060] In an optional embodiment, the channel layer 34 is made of GaN material with a thickness of 20-1000 nm. However, the embodiments of the present disclosure are not limited thereto, and the channel layer 24 may also be made of AlGaN or InGaN material.

[0061] In an optional embodiment, the barrier layer 35 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer 35 may also be an AlN layer, an AlInN layer, AlInGaN, or a plurality of superpositions of the above material layers.

[0062] In an optional embodiment, an AlN insertion layer is further included below the barrier layer, with a thickness of 0.1-2 nm.

[0063] In an optional embodiment, the barrier layer further includes a GaN cap layer with a thickness of 0.1-10 nm, or an in-situ SiN dielectric layer with a thickness of 0.5-150 nm, or a p-type GaN layer with a thickness of 10-200 nm.

[0064] Reference Figure 6a-6c As shown, this embodiment provides a process flow for preparing the nitride semiconductor epitaxial wafer.

[0065] Step 1, such as Figure 6a As shown, a composite substrate 30 is provided, including a lower silicon material layer 301 with a thickness of 670 microns, an intermediate insulating material layer 302 which is an AlN layer with a thickness of 5 microns, and an upper silicon material layer 303 with a thickness of 1 micron.

[0066] Step 2, such as Figure 6b As shown, a transition layer 32 is grown on the substrate. The transition layer in this embodiment is a 3C-SiC single layer grown by vacuum chemical epitaxy, and has a thickness of 50 nm.

[0067] Step 3, such as Figure 6c As shown, the epitaxial wafer after the transition layer 32 is grown is subjected to a wet oxidation process commonly used in silicon processing technology, and water vapor is introduced at high temperature to transform the upper silicon material layer 303 between the insulating material layer AlN302 and the transition layer 32 into an insulating dielectric layer (SiO2) 303'.

[0068] Step 4, such as Figure 6d As shown, after the insulating dielectric layer (SiO2) 303' is grown, a nitride buffer layer is grown on the epitaxial wafer, including a 100nm AlN layer, a 50nm AlGaN layer, and a 3000nm AlN / GaN superlattice structure. A 300nm GaN channel layer, a 1nm AlN insertion layer (not shown in the schematic diagram), a 25nm AlGaN barrier layer, and an 80nm in-situ SiN layer are grown on the buffer layer.

[0069] The above is only a specific implementation of the embodiment of the present invention, but the protection scope of the embodiment of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the embodiment of the present invention, which should be included in the protection scope of the embodiment of the present invention. Therefore, the protection scope of the embodiment of the present invention should be based on the protection scope of the claims.

Claims

1. An epitaxial wafer structure, characterized in that: include: A composite substrate, a transition layer, a buffer layer on the transition layer, a channel layer above the buffer layer, and a barrier layer above the channel layer, wherein the composite substrate is a Si / insulating material / SiO2 structure or a Si / insulating material / Si3N4 structure.

2. A method for preparing an epitaxial wafer, characterized in that: At least for making the epitaxial structure as claimed in claim 1, comprising the following steps: S1. Providing a Si / insulating material / Si structure substrate and growing a transition layer on the substrate; S2, oxidizing or nitriding the silicon material layer between the transition layer and the insulating material in the substrate through an oxidation or nitridation process to form a silicon dioxide or silicon nitride insulating dielectric layer; S3. A buffer layer, a channel layer and a barrier layer are grown in sequence on the transition layer according to a common nitride epitaxial growth process.

3. A method for preparing an epitaxial wafer as claimed in claim 2, characterized in that: Si / insulating material / Si is a Si / SiO2 / Si structure, or a Si / SiN / Si structure, or a Si / AlN / Si structure.

4. A method for preparing an epitaxial wafer as claimed in claim 2, characterized in that: The transition layer is selected from one of the following materials: gallium nitride, aluminum nitride, indium nitride, or alloy materials or multi-layer stacked structures of the above materials; or 3C-SiC material, SiN material; or first growing a layer of 3C-SiC or SiN material on the surface of the silicon substrate, and then continuing to grow the above gallium nitride, aluminum nitride, indium nitride, or alloy materials or multi-layer stacked structures of the above materials.

5. A method for preparing an epitaxial wafer as claimed in claim 2, characterized in that: The oxidation process is selected from one of the following processes: dry oxidation process, wet oxidation process, oxygen ion implantation; The nitridation process is selected from one of the following processes: nitrogen ion implantation; treating the substrate with a nitrogen-containing gas in a high temperature environment; exposing the substrate to a plasma atmosphere containing the N element.

6. A method for preparing an epitaxial wafer as claimed in claim 2, characterized in that: The buffer layer is made of one of the following materials: AlN, AlGaN, a GaN single layer or multi-layer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN super lattice structure, or a combination of the above structures.

7. A method for preparing an epitaxial wafer as claimed in claim 2, characterized in that: The channel layer is selected from one of the following materials: GaN material, AlGaN material, and InGaN material.

8. The method for preparing an epitaxial wafer according to claim 2, characterized in that: The barrier layer is selected from one of the following materials: AlGaN layer, AlN layer, AlInN layer, AlInGaN layer, and a plurality of superpositions of the above material layers.

9. A method for preparing an epitaxial wafer as claimed in claim 2, characterized in that: An AlN insertion layer may be included between the channel layer and the barrier layer.

10. The method for preparing an epitaxial wafer according to claim 2, characterized in that: The barrier layer includes a non-intentionally doped GaN cap layer or an in-situ SiN dielectric layer, or a p-type AlGaInN alloy layer of any proportion.

Citation Information

Cited By

  • Composite substrate nitride epitaxial wafer and preparation method thereof

    CN120690672A

  • Silicon-based indium phosphide laser and preparation method thereof

    CN121566267A