Method for improving interface quality and mobility of SiC Mosfet chip

By employing hydrogen etching and high-temperature N2 nitriding, the problem of high interface defect density in SiC MOSFET chips was solved, enabling the fabrication of SiC MOSFET chips with high mobility and low resistance, thereby reducing costs and environmental pollution.

CN118919402APending Publication Date: 2024-11-08谢雨琳
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311637931.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In existing SiC MOSFET chip manufacturing processes, the high density of SiC interface defects leads to low electron mobility, making it difficult to achieve high performance and high yield.

Method used

Hydrogen etching is used to remove defects on the surface of SiC wafers. After depositing a Si thin film, a SiO2 thin film is formed at low temperature. Then, a high-temperature N2 nitriding treatment is performed to avoid the use of nitric oxide, thereby improving interface quality and mobility.

Benefits of technology

It significantly reduces the defect density at the SiC interface, improves mobility, reduces on-resistance, enhances gate oxide quality, and reduces environmental pollution and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919402A_ABST
    Figure CN118919402A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the interface quality and mobility of a SiC Mosfet chip. The method comprises the following steps: removing defects remaining on the surface of a SiC wafer; depositing a layer of Si film on the surface of the SiC wafer; putting into a furnace tube, adding oxygen, and oxidizing the device at the temperature of 750 DEG C to form a gate oxide SiO2 film; then, the obtained chip is subjected to N2 nitriding treatment, the temperature is set to be 1400-1600 DEG C, and the nitrided chip is cleaned. According to the method, due to the fact that the initial oxidation temperature of Si and the initial oxidation temperature of SiC are different, only a silicon oxide film is oxidized when the temperature reaches 750 DEG C, SiC cannot be oxidized, therefore, no residual C generates defects, the problem of thermal oxidation of SiC Mosfet is solved, the performance of SiC can be improved by 10 times, and the performance of SiC can be improved by 10 times. According to the method, highly toxic nitric oxide is not adopted, heat treatment is carried out in high-temperature N2 gas to improve the interface quality of the chip, and the yield and reliability of the SiC Mosfet chip are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for improving the interface quality and mobility of a SiC Mosfet chip. Background Art

[0002] As newly emerging third-generation semiconductors, silicon carbide (SiC) and gallium nitride have been listed as national frontier science and technology research projects on March 13, 2021. Silicon carbide is a very excellent material with high hardness, corrosion resistance, high temperature resistance, fast heat transfer and good conductivity. The semiconductor power devices made from it have low impedance, low loss, high reliability, high power density, high voltage resistance, high temperature resistance, small size and low system cost. Therefore, its devices and modules can be widely used in new energy, high-speed rail, aviation, robots, laser weapons, rail transit and other fields, especially in electric vehicles / charging piles, energy storage, and photovoltaics.

[0003] Silicon carbide (SiC) has the physical properties of wide bandgap, high breakdown electric field, high thermal conductivity and high electron saturation rate, which makes it resistant to high temperature, high voltage, high frequency, high power and radiation, and can reduce the energy consumption of downstream products and reduce the terminal volume. The bandgap of silicon carbide is about 3.2eV, and the bandgap of silicon is 1.12eV. The bandgap of silicon carbide is 3 times that of silicon. How to reduce the gate oxide interface state density, improve the gate oxide quality and increase the mobility is a global problem in the manufacturing process of SiC Mosfet power chips.

[0004] In the manufacturing process of SiC wafers and transistors, the SiC surface needs to be oxidized. During the thermal oxidation process of silicon carbide Mosfet chips, a SiO2 oxide film will be formed on the surface, which is regarded as a major advantage of SiC. However, during oxidation, residual carbon will precipitate from the SiC interface, resulting in interface defects that are 100 times larger than Si. This high defect density causes the electron mobility of SiC to decrease, thereby increasing resistance, so the high performance and yield improvement that SiC should have cannot be achieved. It is crucial to remove these defects.

[0005] At present, the standard gate oxide process for SiC Mosfet production is: entering the furnace tube, generating SiO2 film through thermal oxidation process, and then reducing the interface defects between SiO2 and SiC Mosfet chip through highly toxic nitric oxide (NO) gas treatment. In fact, SiC Mosfet chip will be oxidized by oxygen atoms in nitric oxide, thus generating new defects. Therefore, this traditional method has limited effect on improving SiC interface quality. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art, break the existing SiC Mosft chip processing process, and provide a method for improving the interface quality and mobility of SiC Mosfet chips. The method of the present invention can reduce the interface state density of SiC Mosfet chips, improve the channel mobility, reduce the on-resistance of SiC Mosfet chips, enhance the gate oxide quality of SiC Mosfet chips and improve the yield.

[0007] The object of the present invention is achieved in that:

[0008] A method for improving the interface quality and mobility of a SiC Mosfet chip comprises the following steps:

[0009] S1. Remove the defects remaining on the surface of SiC Mosfet wafer by etching;

[0010] S2, depositing a layer of Si film on the surface of SiC Mosfet wafer;

[0011] S3, placing the chip in step S2 into a furnace tube, adding oxygen, and oxidizing the chip at a temperature of 750° C. to form a gate oxide SiO2 film on the surface of the SiC wafer;

[0012] S4, performing nitridation treatment on the chip obtained in step S3, with the temperature set within 1400° C.-1600° C.;

[0013] S5. Cleaning the chip after nitridation treatment.

[0014] Furthermore, the etching method in S1 is hydrogen etching.

[0015] Furthermore, in S2, Si is deposited on the surface of the SiC Mosfet wafer by chemical vapor deposition.

[0016] Furthermore, the deposition thickness of the Si film in S2 is adjusted according to the required gate oxide thickness.

[0017] Furthermore, the deposition thickness of the Si film is 20nm-30nm. :

[0018] Furthermore, the thickness of the SiO2 film in S3 is 40nm-50nm.

[0019] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:

[0020] 1. Before forming an oxide film on the surface of the SiC Mosfet wafer, the defects remaining on the surface of the SiC wafer are removed by hydrogen etching.

[0021] 2. Instead of using the traditional SiC Mosfet process to perform thermal oxidation to form the SiO2 film, Si is deposited on the SiC Mosfet wafer by the CVD (chemical vapor deposition) method.

[0022] 3. Taking advantage of the different oxidation starting temperatures of Si and SiC, the oxidation temperature is controlled at 750°C. When the temperature reaches 750°C, only the silicon film is oxidized without oxidizing SiC. Therefore, no residual C is generated on the surface of the SiC wafer, reducing the surface defects of the SiC wafer.

[0023] 4. In the current mass production of SiC Mosfet, highly toxic nitric oxide is needed to nitride the oxidized chips. SiC will be oxidized by the oxygen atoms in the nitric oxide, thereby generating new defects. The method of the present invention avoids the use of nitric oxide and adopts high-temperature N2 gas for heat treatment, thereby improving the interface quality of SiC and SiO2.

[0024] 5. It can reduce the SiC interface defect density from the traditional 1.3×10 11 cm -2 Reduced to 1.2×10 10 cm -2 .

[0025] 6. Compared with the original nitric oxide (NO) gas treatment method, the nitriding treatment reduces the highly toxic pollution and treatment and reduces the process cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the production flow chart of existing SiC Mosfet chips;

[0027] Figure 2 is a flow chart of the method of the present invention;

[0028] Figure 3 The comparison between the method of the present invention and the existing method in reducing SiC / SiO2 interface defects;

[0029] Figure 4 The present invention is compared with the existing method in improving the channel mobility of SiC / SiO2 interface. DETAILED DESCRIPTION

[0030] The technology and features of the present invention are described in detail below through embodiments in conjunction with the accompanying drawings.

[0031] Embodiment 1, a method for improving the interface quality and mobility of SiC Mosfet chip, adopts the following process:

[0032] 1. Before the SiC Mosfet chip is transferred to the gate oxide step according to the existing production process, before the oxide film is formed on the surface of the SiC wafer, the defects remaining on the surface of the SiC wafer are removed by hydrogen etching;

[0033] 2. Deposit a 20nm silicon film on the surface of the SiC wafer by CVD (chemical vapor deposition) method. The thickness of the silicon film can also be defined according to the required gate oxide thickness;

[0034] 3. Place the deposited SiC Mosfet chip wafer into the furnace tube, add oxygen at low temperature, and oxidize the chip at 750°C to convert the silicon film into a SiO2 film with a thickness of 40nm. Since the oxidation starting temperature of silicon is 700°C and the oxidation starting temperature of SiC is 900°C, only the silicon film will be oxidized at 750°C without oxidizing SiC, so that there is no residual C on the interface of the SiC Mosfet chip, thereby reducing the interface defects of SiC and SiO2;

[0035] 4. After oxidation, N2 nitridation treatment is carried out at a high temperature of 1400°C. The use of N2 nitridation treatment can prevent SiC from being oxidized by oxygen atoms in nitric oxide, reduce interface defects between SiO2 and SiC, and improve interface quality;

[0036] 5. Clean the chip after nitridation treatment.

[0037] After the above steps, the interface defect density of SiC Mosfet chip can reach 1.28×10 10 cm -2 , the migration rate reaches 74cm 2 / Vs;

[0038] In Example 2, the deposition thickness of the silicon film is set to 30 nm, the thickness of the silicon film after oxidation is 50 nm, the N2 nitridation treatment temperature is set to 1600 ° C, and the remaining steps are the same as in Example 1. After the treatment, the interface defect density of the chip reaches 1.2×10 10 cm -2 , the mobility reaches 82cm 2 / Vs;

[0039] like Figure 3 , Figure 4 As shown, Figure 3 The figure shows a comparison of the interface defect density of SiC / SiO2 obtained by the process method of the present invention and the existing process method. It can be seen from the figure that the interface defect value of SiC and SiO2 treated with N2 in the present invention is much lower than the interface defect value treated with NO, and SiC / SiO2 is not oxidized by the oxygen atoms in NO during the treatment process, thereby reducing the defects of the SiCMosfet chip.

[0040] Figure 4 The figure shows the comparison of the chip channel mobility obtained by the process method of the present invention and the existing process method. It can be seen from the figure that the chip mobility after NO treatment in the prior art can reach 40cm at best. 2 / Vs, this value cannot meet the requirements of silicon carbide power device manufacturing yield and device automotive-grade reliability, and is far from the theoretical value. However, the chip mobility after treatment by the method of the present invention can reach 80cm 2 / Vs, which is much higher than the mobility of existing products.

[0041] The method of the present invention can reduce the defect density of the chip from the traditional 1.3×10 11 cm -2 Reduced to 1.2×10 10 cm -2 About one tenth, since the number of defects is proportional to the performance, it means that the performance of SiC has been improved by 10 times. In addition, the insulation of SiO2 film is excellent, and its dielectric breakdown strength reaches 10MV / cm. Compared with the traditional SiC Mosfet oxide film, the voltage stress resistance and reliability are also improved, so the interface state density is effectively reduced, the mobility is improved, and the on-resistance is reduced. The gate oxide quality is greatly improved, and the cost of SiC chips can be reduced to 30%-50% of the traditional method. At the same time, the NO treatment process is cancelled, which reduces costs while reducing pollution to the environment.

[0042] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A method for improving the interface quality and mobility of SiC Mosfet chips, characterized in that: The following steps are involved: S1. Remove the defects remaining on the surface of the SiC wafer by etching; S2, depositing a layer of Si film on the surface of the SiC wafer; S3, placing the device in step S2 into a furnace tube, adding oxygen, and oxidizing the chip at a temperature of 750° C. to form a gate oxide SiO2 film on the surface of the SiC wafer; S4, performing nitridation treatment on the chip obtained in step S3, with the temperature set within 1400° C.-1600° C.; S5. Cleaning the chip after nitridation treatment.

2. A method for improving the interface quality and mobility of SiC chips according to claim 1, characterized in that: The etching method in S1 is hydrogen etching.

3. A method for improving the interface quality and mobility of SiC Mosfet chips according to claim 1, characterized in that: In S2, Si is deposited on the surface of the SiC Mosfet wafer by chemical vapor deposition.

4. A method for improving the interface quality and mobility of SiC Mosfet chips according to any one of claims 1 or 3, characterized in that: The deposition thickness of the Si film in S2 is adjusted according to the required gate oxide thickness.

5. A method for improving SiC Mosfet interface quality and mobility according to claim 4, characterized in that: The deposition thickness of the Si film is 20nm-30nm.

6. A method for improving the interface quality and mobility of SiC Mosfet chips according to claim 5, characterized in that: The thickness of SiO2 film in S3 is 40nm-50nm.