Groove MIS structure transistor with tooth-shaped p-GaN buried layer
By setting a toothed p-GaN buried layer between the source and drain and a groove structure below the gate electrode trench in the GaN buffer layer, the electric field distribution of the p-GaN HEMT device is improved, the problem of insufficient threshold voltage and breakdown voltage is solved, and the reliability and performance of the device are improved.
Patent Information
- Application Number
- CN202411004139.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-25
Smart Images

Figure CN118919553A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wide bandgap semiconductor materials and devices, and in particular to a groove MIS structure transistor with a toothed p-GaN buried layer. Background Art
[0002] Gallium nitride (GaN) materials have the characteristics of wide bandgap and high temperature resistance, which enables AlGaN / GaN HEMT devices to work normally in high temperature, strong electric field, high frequency and high power environment without affecting the device characteristics. At present, it has been greatly developed in the fields of new energy, electric vehicles, 5G communications, etc.
[0003] The p-GaN gate HEMT device realizes an enhancement mode device by growing a p-type doped GaN layer between the gate electrode and the AlGaN barrier layer, which can obtain a positive threshold voltage. It has the advantages of simple preparation process and small etching damage, but its too low threshold voltage and low breakdown voltage when the device is turned off require the design of a special drive circuit to ensure the normal operation of the device. Therefore, improving the threshold voltage and breakdown voltage of the p-GaN HEMT device, increasing the current of the device, and improving the reliability of the device are still problems that need to be solved.
[0004] In the prior art, GaN HEMT devices can use field plate technology, ion implantation technology, gate edge etching technology and other methods to improve the device's breakdown voltage, and groove structures and other methods can improve the device's threshold voltage characteristics, etc. The patent application with publication number CN107170671A discloses a GaN power device based on ion implantation and a manufacturing method thereof. Its gate edge etching technology and field plate technology can only alleviate the local peak electric field at the edge of the gate electrode, but cannot alleviate the overall electric field change and average electric field between the source and drain of the device, and the voltage resistance improvement of the device is limited. The ion implantation technology will damage the channel layer of the device, thereby affecting the voltage resistance performance of the device, reducing the reliability of the device, and limiting the performance of the device. Summary of the invention
[0005] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a groove MIS structure transistor with a toothed p-GaN buried layer. A toothed source-drain p-GaN buried layer is arranged in a GaN buffer layer, which can improve the electric field distribution between the gate and drain, between the gate and source, and between the source and drain of the device, and reduce the average electric field size. Compared with the previous method, the present invention has a better electric field relief effect, increases the breakdown voltage of the device, and makes the device more difficult to be broken down; secondly, a groove structure is formed by etching the barrier layer in the area below the gate, a p-GaN layer is deposited above the groove, and a gate dielectric layer is grown between the groove p-GaN layer and the gate electrode to obtain a high threshold voltage and a large current, reduce the gate leakage of the device, and at the same time improve the gate's voltage resistance, improve the switching speed of the device, and improve the reliability of the device.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A groove MIS structure transistor with a toothed p-GaN buried layer comprises a substrate 1, a nucleation layer 2, a first GaN buffer layer 3, a source-drain p-GaN buried layer 4, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 which are sequentially arranged from bottom to top; a drain electrode 13 and a source electrode 12 are respectively arranged on both sides of the AlGaN barrier layer 7, a gate electrode groove 8 is arranged on the side of the AlGaN barrier layer 7 close to the drain electrode 13, and a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 which are arranged from bottom to top are arranged in the gate electrode groove 8; toothed protrusions and grooves matching the protrusions are distributed on the opposite sides of the first GaN buffer layer 3 and the second GaN buffer layer 5, the source-drain p-GaN buried layer 4 is located between the first GaN buffer layer 3 and the second GaN buffer layer 5, and the shape of the contact surface between the source-drain p-GaN buried layer 4 and the first GaN buffer layer 3 and the second GaN buffer layer 5 is matched.
[0008] The tooth-like protrusions and grooves on the opposite surfaces of the first GaN buffer layer 3 and the second GaN buffer layer 5 are in a square, arc, cone, trapezoid or step shape; the thickness of the p-GaN buried layer 4 between the source and the drain is 150nm to 300nm.
[0009] The cone tip angle of the cone is 30° to 60°, the inclination angle of the trapezoid is 45° to 90°, and the step inclination angle of the step shape is 45° to 60°.
[0010] The gate electrode 11 is a Schottky contact, the source electrode 12 and the drain electrode 13 are in contact with the AlGaN barrier layer 7 respectively, and the source electrode 12 and the drain electrode 13 are not connected to each other.
[0011] The source electrode 12 and the drain electrode 13 both use Ti as the base metal, and are formed by integrally solidifying Ti, Al, Ni and Au from bottom to top, wherein Ti metal is the barrier layer metal, and Ti diffuses into the AlGaN barrier layer 7 to form TiN with low work function and generate nitrogen vacancies, thereby forming an ohmic contact.
[0012] The gate electrode groove 8 has a depth of 20 nm to 25 nm.
[0013] The p-type doping concentration of the p-GaN buried layer 4 between the source and drain is 3e 16 cm -3 ~8e 17 cm -3 ; The p-type doping concentration in the p-GaN layer 9 is 5e 17 cm -3 ~7e 17 cm -3 .
[0014] The nucleation layer 2 is composed of an AlGaN layer with a gradient Al component, and the Al 0.2 Ga 0.8 N, 150nm~200nm thick Al 0.5 Ga 0.5 N and 150nm~200nm thick Al 0.8 Ga 0.2 N.
[0015] The gate electrode 11 is 3.5-4.0 μm long, the distance between the source electrode and the drain electrode is 10-15 μm, the distance between the gate electrode and the source electrode is 1-2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm-10 μm.
[0016] The gate dielectric layer 10 is made of a high dielectric constant dielectric material, including Al2O3 and AlN.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The present invention sets a toothed source-drain p-GaN buried layer 4 in the GaN buffer layer, which can improve the electric field distribution between the gate and drain, between the gate and source, and between the source and drain of the device, and reduce the average electric field size. Compared with the previous method, the present invention has a better electric field relief effect, increases the breakdown voltage of the device, and makes the device more difficult to be broken down.
[0019] 2. By providing a toothed source-drain p-GaN buried layer 4 in the first GaN buffer layer, the carrier concentration can be increased, lattice defects can be reduced, lattice quality can be improved, carrier mobility can be improved, and the electric field distribution between the gate and drain, between the gate and source, and between the source and drain of the device can be improved, thereby reducing the average electric field size. Compared with technologies such as gate edge, this method can alleviate the electric field distribution of the entire device, has a better effect on electric field relief, is conducive to increasing the breakdown voltage of the device, and makes the device more difficult to be broken down. Compared with conventional p-GaN gate HEMT devices without a p-GaN buried layer 4 structure between the source and drain, the breakdown voltage of the device of the present invention can reach 1421V, which greatly improves the breakdown voltage of the device. Secondly, a groove structure is formed by etching the barrier layer in the area below the gate, and a p-GaN layer is deposited above the groove to better deplete the two-dimensional electron gas (2DEG) below to obtain an enhanced device.
[0020] 3. The present invention forms a groove structure by etching the AlGaN barrier layer 7 in the area below the gate, and deposits a p-GaN layer 9 above the gate electrode groove 8 to better deplete the two-dimensional electron gas (2DEG) below, thereby obtaining an enhanced device. The gate dielectric layer 10 grown between the groove p-GaN layer 9 and the gate electrode 11 is used to obtain a high threshold voltage and a large current, reduce the gate leakage of the device, and at the same time improve the gate's voltage resistance, improve the switching speed of the device, and improve the reliability of the device. Compared with conventional devices, the breakdown voltage of the device of the present invention can reach 1421V, which simplifies the process flow during the device process preparation and reduces the manufacturing cost.
[0021] 4. In the preparation of the present invention, a gate dielectric layer 10 is used between the p-GaN layer 9 in the groove and the gate electrode 11 to obtain a high threshold voltage and a large current, reduce the gate leakage of the device, and at the same time improve the voltage resistance of the gate electrode, increase the switching speed of the device, and thus improve the reliability of the device during operation.
[0022] 5. The nucleation layer 2 of the present invention is composed of an AlGaN layer with a gradient Al component; it avoids the problems of lattice mismatch, many dislocation defects, etc. when the GaN layer is directly grown on the substrate, which affects the epitaxial effect of the subsequent GaN layer; after adding the AlGaN layer with a gradient Al component as the nucleation layer, the present invention improves the wettability between the GaN buffer layer and the substrate, reduces the lattice mismatch phenomenon, and reduces defects such as dislocations, thereby obtaining a high-quality GaN epitaxial layer, which can minimize the lattice mismatch and stress problems in the material epitaxial process, and is beneficial to controlling the quality and stress of the GaN epitaxial layer.
[0023] In summary, the present invention has the advantages of increasing the breakdown voltage of the device, reducing the leakage current of the device, significantly increasing the threshold voltage of the device, obtaining a large current, suppressing the gate leakage phenomenon of the device, and at the same time improving the voltage resistance of the gate electrode and the switching speed of the device, thereby improving the working reliability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the device structure of Example 1 of the present invention.
[0025] Figure 2 Schematic diagram of two different concentration distributions of the p-GaN buried layer 4 in Example 1 of the present invention.
[0026] Figure 3 It is a schematic diagram of forming a groove MIS structure transistor with a toothed p-GaN buried layer according to the present invention.
[0027] Figure 4 It is a schematic diagram of the device structure of Example 2 of the present invention.
[0028] Figure 5 It is a schematic diagram of the device structure of Example 3 of the present invention.
[0029] Figure 6 It is a schematic diagram of the device structure of Example 4 of the present invention.
[0030] Figure 7 It is a schematic diagram of the device structure of Example 5 of the present invention.
[0031] Figure 8 It is a schematic diagram of the breakdown characteristics of the transistor with a groove MIS structure having a toothed p-GaN buried layer according to the present invention.
[0032] In the figure: 1. substrate; 2. nucleation layer; 3. first GaN buffer layer; 4. p-GaN buried layer between source and drain; 5. second GaN buffer layer; 6. GaN layer; 7. AlGaN barrier layer; 8. gate electrode groove; 9. p-GaN layer; 10. gate dielectric layer; 11. gate electrode; 12. source electrode; 13. drain electrode. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below with reference to the accompanying drawings.
[0034] Example 1
[0035] like Figure 1As shown, a groove MIS structure transistor with a toothed p-GaN buried layer comprises a substrate 1, a nucleation layer 2, a first GaN buffer layer 3, a p-GaN buried layer 4 between source and drain, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 which are sequentially arranged from bottom to top; a drain electrode 13 and a source electrode 12 are respectively arranged on both sides of the AlGaN barrier layer 7, a gate electrode groove 8 is arranged on the side of the AlGaN barrier layer 7 close to the drain electrode 13, and a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 which are arranged from bottom to top are arranged in the gate electrode groove 8; toothed protrusions and grooves which match the protrusions are distributed on the opposite sides of the first GaN buffer layer 3 and the second GaN buffer layer 5, the p-GaN buried layer 4 between source and drain is located between the first GaN buffer layer 3 and the second GaN buffer layer 5, and the shape of the contact surface between the p-GaN buried layer 4 between source and drain matches the shape of the contact surface between the first GaN buffer layer 3 and the second GaN buffer layer 5.
[0036] The tooth-like protrusions and grooves on the opposite surfaces of the first GaN buffer layer 3 and the second GaN buffer layer 5 are square; the thickness of the p-GaN buried layer 4 between the source and the drain is 200 nm.
[0037] The first GaN buffer layer 3 is 5 μm thick, the p-GaN buried layer 4 between the source and drain is 200 nm thick, the second GaN buffer layer 5 is 45 μm thick, the GaN layer 6 is 100 nm thick, the AlGaN barrier layer 7 is 60 nm thick, the p-GaN layer 9 is 120 nm thick, and the gate dielectric layer 10 is 20 nm thick.
[0038] The gate electrode 11 is a Schottky contact, the source electrode 12 and the drain electrode 13 are in contact with the AlGaN barrier layer 7 respectively, and the source electrode 12 and the drain electrode 13 are not connected to each other.
[0039] The source electrode 12 and the drain electrode 13 are both made of Ti as the base metal, and are formed by the overall solidification of Ti, Al, Ni and Au from bottom to top. Among them, Ti metal is the barrier layer metal, and Ti diffuses into the AlGaN barrier layer 7 to form TiN with low work function and generate a large number of nitrogen vacancies, thereby forming an ohmic contact. The thicknesses of Ti, Al, Ni and Au are 40nm, 80nm, 40nm and 120nm respectively. Metal Al is the cover layer metal and acts as a catalyst to promote Ti and the nitrogen element in GaN to form TiN; Ni and Au belong to the cap layer metal. Ni prevents the upper layer Au from diffusing downward, and Au plays a protective role to prevent the metal below from being oxidized.
[0040] The gate electrode groove 8 has a depth of 25 nm.
[0041] The p-type doping concentration of the p-GaN buried layer 4 between the source and drain is 3e 16 cm -3 ; The p-type doping concentration in the p-GaN layer 9 is 5e17 cm -3 .
[0042] The nucleation layer 2 is composed of AlGaN with a gradient Al component, and the Al 0.2 Ga 0.8 N, 200nm thick Al 0.5 Ga 0.5 N and 200nm thick Al 0.8 Ga 0.2 N; the nucleation layer can minimize the lattice mismatch and stress problems in the material epitaxial process, which is beneficial to controlling the quality and stress of the GaN epitaxial layer.
[0043] The gate electrode 11 is 3.5 μm long, the distance between the source electrode and the drain electrode is 15 μm, the distance between the gate electrode and the source electrode is 2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm.
[0044] The gate dielectric layer 10 is made of Al2O3.
[0045] like Figure 2 As shown, increasing the thickness of the p-GaN buried layer 4 between the source and drain and the p-type doping concentration (uniform concentration, high doping step concentration) at different locations can improve the overall performance of the device, including improving the electric field distribution, increasing the breakdown voltage, reducing leakage, etc.
[0046] like Figure 3 The figure shows the preparation process of the device of the present invention, providing a substrate 1, and depositing a nucleation layer 2, a first GaN buffer layer 3, a p-GaN buried layer 4 between source and drain, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 on the substrate 1 in sequence; the toothed contact surfaces of the first GaN buffer layer 3, the p-GaN buried layer 4 between source and drain and the second GaN buffer layer 5 are formed by etching, a gate electrode groove 8 and a source electrode region and a drain electrode region are etched on the AlGaN barrier layer 7, a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 are deposited in the gate electrode groove 8 in sequence, and the source electrode region and the drain electrode region are solidified as a whole using Ti, Al, Ni and Au in sequence from bottom to top.
[0047] Example 2
[0048] A groove MIS structure transistor with a toothed p-GaN buried layer comprises a substrate 1, a nucleation layer 2, a first GaN buffer layer 3, a source-drain p-GaN buried layer 4, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 which are sequentially arranged from bottom to top; a drain electrode 13 and a source electrode 12 are respectively arranged on both sides of the AlGaN barrier layer 7, a gate electrode groove 8 is arranged on the side of the AlGaN barrier layer 7 close to the drain electrode 13, and a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 which are arranged from bottom to top are arranged in the gate electrode groove 8; toothed protrusions and grooves matching the protrusions are distributed on the opposite sides of the first GaN buffer layer 3 and the second GaN buffer layer 5, the source-drain p-GaN buried layer 4 is located between the first GaN buffer layer 3 and the second GaN buffer layer 5, and the shape of the contact surface between the source-drain p-GaN buried layer 4 and the first GaN buffer layer 3 and the second GaN buffer layer 5 is matched.
[0049] The tooth-like protrusions and grooves on the opposite surfaces of the first GaN buffer layer 3 and the second GaN buffer layer 5 are square; the thickness of the p-GaN buried layer 4 between the source and the drain is 250 nm.
[0050] The first GaN buffer layer 3 is 5 μm thick, the p-GaN buried layer 4 between the source and drain is 250 nm thick, the second GaN buffer layer 5 is 45 μm thick, the GaN layer 6 is 100 nm thick, the AlGaN barrier layer 7 is 60 nm thick, the p-GaN layer 9 is 120 nm thick, and the gate dielectric layer 10 is 20 nm thick.
[0051] The gate electrode 11 is a Schottky contact, the source electrode 12 and the drain electrode 13 are in contact with the AlGaN barrier layer 7 respectively, and the source electrode 12 and the drain electrode 13 are not connected to each other.
[0052] The source electrode 12 and the drain electrode 13 are both made of Ti as the base metal, and are formed by the overall solidification of Ti, Al, Ni and Au from bottom to top. Among them, Ti metal is the barrier layer metal, and Ti diffuses into the AlGaN barrier layer 7 to form TiN with low work function and generate a large number of nitrogen vacancies, thereby forming an ohmic contact. The thicknesses of Ti, Al, Ni and Au are 40nm, 80nm, 40nm and 120nm respectively. Metal Al is the cover layer metal and acts as a catalyst to promote Ti and the nitrogen element in GaN to form TiN; Ni and Au belong to the cap layer metal. Ni prevents the upper layer Au from diffusing downward, and Au plays a protective role to prevent the metal below from being oxidized.
[0053] The gate electrode groove 8 has a depth of 20 nm.
[0054] The p-type doping concentration of the p-GaN buried layer 4 between the source and drain is 8e 17 cm -3 ; The p-type doping concentration in the p-GaN layer 9 is 7e 17cm -3 .
[0055] The nucleation layer 2 is composed of AlGaN with a gradient Al component, and the Al 0.2 Ga 0.8 N, 200nm thick Al 0.5 Ga 0.5 N and 200nm thick Al 0.8 Ga 0.2 N; the nucleation layer can minimize the lattice mismatch and stress problems in the material epitaxial process, which is beneficial to controlling the quality and stress of the GaN epitaxial layer.
[0056] The gate electrode 11 is 3.5 μm long, the distance between the source electrode and the drain electrode is 15 μm, the distance between the gate electrode and the source electrode is 2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm.
[0057] The gate dielectric layer 10 is made of AlN.
[0058] Example 3
[0059] A groove MIS structure transistor with a toothed p-GaN buried layer comprises a substrate 1, a nucleation layer 2, a first GaN buffer layer 3, a source-drain p-GaN buried layer 4, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 which are sequentially arranged from bottom to top; a drain electrode 13 and a source electrode 12 are respectively arranged on both sides of the AlGaN barrier layer 7, a gate electrode groove 8 is arranged on the side of the AlGaN barrier layer 7 close to the drain electrode 13, and a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 which are arranged from bottom to top are arranged in the gate electrode groove 8; toothed protrusions and grooves matching the protrusions are distributed on the opposite sides of the first GaN buffer layer 3 and the second GaN buffer layer 5, the source-drain p-GaN buried layer 4 is located between the first GaN buffer layer 3 and the second GaN buffer layer 5, and the shape of the contact surface between the source-drain p-GaN buried layer 4 and the first GaN buffer layer 3 and the second GaN buffer layer 5 is matched.
[0060] The tooth-like protrusions and grooves on the opposite surfaces of the first GaN buffer layer 3 and the second GaN buffer layer 5 are arc-shaped; the thickness of the p-GaN buried layer 4 between the source and the drain is 300 nm.
[0061] The first GaN buffer layer 3 is 5 μm thick, the p-GaN buried layer 4 between the source and drain is 300 nm thick, the second GaN buffer layer 5 is 45 μm thick, the GaN layer 6 is 100 nm thick, the AlGaN barrier layer 7 is 60 nm thick, the p-GaN layer 9 is 120 nm thick, and the gate dielectric layer 10 is 20 nm thick.
[0062] The gate electrode 11 is a Schottky contact, the source electrode 12 and the drain electrode 13 are in contact with the AlGaN barrier layer 7 respectively, and the source electrode 12 and the drain electrode 13 are not connected to each other.
[0063] The source electrode 12 and the drain electrode 13 are both made of Ti as the base metal, and are formed by the overall solidification of Ti, Al, Ni and Au from bottom to top. Among them, Ti metal is the barrier layer metal, and Ti diffuses into the AlGaN barrier layer 7 to form TiN with low work function and generate a large number of nitrogen vacancies, thereby forming an ohmic contact. The thicknesses of Ti, Al, Ni and Au are 40nm, 80nm, 40nm and 120nm respectively. Metal Al is the cover layer metal and acts as a catalyst to promote Ti and the nitrogen element in GaN to form TiN; Ni and Au belong to the cap layer metal. Ni prevents the upper layer Au from diffusing downward, and Au plays a protective role to prevent the metal below from being oxidized.
[0064] The gate electrode groove 8 has a depth of 25 nm.
[0065] The p-type doping concentration of the p-GaN buried layer 4 between the source and drain is 3e 16 cm -3 ; The p-type doping concentration in the p-GaN layer 9 is 5e 17 cm -3 .
[0066] The nucleation layer 2 is composed of AlGaN with a gradient Al component, and the Al 0.2 Ga 0.8 N, 200nm thick Al 0.5 Ga 0.5 N and 200nm thick Al 0.8 Ga 0.2 N; the nucleation layer can minimize the lattice mismatch and stress problems in the material epitaxial process, which is beneficial to controlling the quality and stress of the GaN epitaxial layer.
[0067] The gate electrode 11 is 3.5 μm long, the distance between the source electrode and the drain electrode is 15 μm, the distance between the gate electrode and the source electrode is 2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm.
[0068] The gate dielectric layer 10 is made of Al2O3.
[0069] like Figure 4 As shown, the difference between this example and Example 1 and Example 2 is that the p-GaN buried layer 4 between the source and drain described in this example is an arc-shaped strip structure. The arc-shaped strip structure is closer to the electric field distribution under the gate electrode, and both are divergent, which is beneficial to reduce the overall electric field peak between the gate and drain, improve the electric field distribution, and help increase the breakdown voltage.
[0070] Example 4
[0071] A groove MIS structure transistor with a toothed p-GaN buried layer comprises a substrate 1, a nucleation layer 2, a first GaN buffer layer 3, a source-drain p-GaN buried layer 4, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 which are sequentially arranged from bottom to top; a drain electrode 13 and a source electrode 12 are respectively arranged on both sides of the AlGaN barrier layer 7, a gate electrode groove 8 is arranged on the side of the AlGaN barrier layer 7 close to the drain electrode 13, and a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 which are arranged from bottom to top are arranged in the gate electrode groove 8; toothed protrusions and grooves matching the protrusions are distributed on the opposite sides of the first GaN buffer layer 3 and the second GaN buffer layer 5, the source-drain p-GaN buried layer 4 is located between the first GaN buffer layer 3 and the second GaN buffer layer 5, and the shape of the contact surface between the source-drain p-GaN buried layer 4 and the first GaN buffer layer 3 and the second GaN buffer layer 5 is matched.
[0072] The tooth-like protrusions and grooves on the opposite surfaces of the first GaN buffer layer 3 and the second GaN buffer layer 5 are trapezoidal; the thickness of the p-GaN buried layer 4 between the source and the drain is 250 nm.
[0073] The first GaN buffer layer 3 is 5 μm thick, the p-GaN buried layer 4 between the source and drain is 250 nm thick, the second GaN buffer layer 5 is 45 μm thick, the GaN layer 6 is 100 nm thick, the AlGaN barrier layer 7 is 60 nm thick, the p-GaN layer 9 is 120 nm thick, and the gate dielectric layer 10 is 20 nm thick.
[0074] The inclination angle of the trapezoid is 75°.
[0075] The gate electrode 11 is a Schottky contact, the source electrode 12 and the drain electrode 13 are in contact with the AlGaN barrier layer 7 respectively, and the source electrode 12 and the drain electrode 13 are not connected to each other.
[0076] The source electrode 12 and the drain electrode 13 are both made of Ti as the base metal, and are formed by the overall solidification of Ti, Al, Ni and Au from bottom to top. Among them, Ti metal is the barrier layer metal, and Ti diffuses into the AlGaN barrier layer 7 to form TiN with low work function and generate a large number of nitrogen vacancies, thereby forming an ohmic contact. The thicknesses of Ti, Al, Ni and Au are 40nm, 80nm, 40nm and 120nm respectively. Metal Al is the cover layer metal and acts as a catalyst to promote Ti and the nitrogen element in GaN to form TiN; Ni and Au belong to the cap layer metal. Ni prevents the upper layer Au from diffusing downward, and Au plays a protective role to prevent the metal below from being oxidized.
[0077] The gate electrode groove 8 has a depth of 25 nm.
[0078] The p-type doping concentration of the p-GaN buried layer 4 between the source and drain is 8e 17 cm -3 ; The p-type doping concentration in the p-GaN layer 9 is 7e 17 cm -3 .
[0079] The nucleation layer 2 is composed of AlGaN with a gradient Al component, and the Al 0.2 Ga 0.8 N, 200nm thick Al 0.5 Ga 0.5 N and 200nm thick Al 0.8 Ga 0.2 N; the nucleation layer can minimize the lattice mismatch and stress problems in the material epitaxial process, which is beneficial to controlling the quality and stress of the GaN epitaxial layer.
[0080] The gate electrode 11 is 3.5 μm long, the distance between the source electrode and the drain electrode is 15 μm, the distance between the gate electrode and the source electrode is 2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm.
[0081] The gate dielectric layer 10 is made of AlN.
[0082] like Figure 5 As shown, the difference between this example and Example 1 is that the p-GaN buried layer 4 between the source and drain described in this example is a trapezoidal strip structure, each p-GaN block is spaced 1 μm apart, the thickness of the p-GaN buried layer 4 between the source and drain is 250 nm, and the trapezoidal inclination angle is 75°. The trapezoidal strip structure alleviates the electric field concentration effect between the gate and source, improves the breakdown characteristics of the device, and enhances the reliability of the device.
[0083] Example 5
[0084] A groove MIS structure transistor with a toothed p-GaN buried layer comprises a substrate 1, a nucleation layer 2, a first GaN buffer layer 3, a source-drain p-GaN buried layer 4, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 which are sequentially arranged from bottom to top; a drain electrode 13 and a source electrode 12 are respectively arranged on both sides of the AlGaN barrier layer 7, a gate electrode groove 8 is arranged on the side of the AlGaN barrier layer 7 close to the drain electrode 13, and a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 which are arranged from bottom to top are arranged in the gate electrode groove 8; toothed protrusions and grooves matching the protrusions are distributed on the opposite sides of the first GaN buffer layer 3 and the second GaN buffer layer 5, the source-drain p-GaN buried layer 4 is located between the first GaN buffer layer 3 and the second GaN buffer layer 5, and the shape of the contact surface between the source-drain p-GaN buried layer 4 and the first GaN buffer layer 3 and the second GaN buffer layer 5 is matched.
[0085] The tooth-like protrusions and grooves on the opposite surfaces of the first GaN buffer layer 3 and the second GaN buffer layer 5 are conical; the thickness of the p-GaN buried layer 4 between the source and the drain is 300 nm.
[0086] The first GaN buffer layer 3 is 5 μm thick, the p-GaN buried layer 4 between the source and drain is 300 nm thick, the second GaN buffer layer 5 is 45 μm thick, the GaN layer 6 is 100 nm thick, the AlGaN barrier layer 7 is 60 nm thick, the p-GaN layer 9 is 120 nm thick, and the gate dielectric layer 10 is 20 nm thick.
[0087] The cone tip angle is 60°
[0088] The gate electrode 11 is a Schottky contact, the source electrode 12 and the drain electrode 13 are in contact with the AlGaN barrier layer 7 respectively, and the source electrode 12 and the drain electrode 13 are not connected to each other.
[0089] The source electrode 12 and the drain electrode 13 are both made of Ti as the base metal, and are formed by the overall solidification of Ti, Al, Ni and Au from bottom to top. Among them, Ti metal is the barrier layer metal, and Ti diffuses into the AlGaN barrier layer 7 to form TiN with low work function and generate a large number of nitrogen vacancies, thereby forming an ohmic contact. The thicknesses of Ti, Al, Ni and Au are 40nm, 80nm, 40nm and 120nm respectively. Metal Al is the cover layer metal and acts as a catalyst to promote Ti and the nitrogen element in GaN to form TiN; Ni and Au belong to the cap layer metal. Ni prevents the upper layer Au from diffusing downward, and Au plays a protective role to prevent the metal below from being oxidized.
[0090] The gate electrode groove 8 has a depth of 20 nm.
[0091] The p-type doping concentration of the p-GaN buried layer 4 between the source and drain is 3e 16 cm -3 ; The p-type doping concentration in the p-GaN layer 9 is 5e 17 cm -3 .
[0092] The nucleation layer 2 is composed of AlGaN with a gradient Al component, and the Al 0.2 Ga 0.8 N, 200nm thick Al 0.5 Ga 0.5 N and 200nm thick Al 0.8 Ga 0.2 N; the nucleation layer can minimize the lattice mismatch and stress problems in the material epitaxial process, which is beneficial to controlling the quality and stress of the GaN epitaxial layer.
[0093] The gate electrode 11 is 3.5 μm long, the distance between the source electrode and the drain electrode is 15 μm, the distance between the gate electrode and the source electrode is 2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm.
[0094] The gate dielectric layer 10 is made of Al2O3.
[0095] like Figure 6 As shown, the difference between this example and Example 1 is that the p-GaN buried layer 4 between the source and drain in this example is a conical band structure, the interval between each p-GaN piece is 0.8 μm, and the angle of the cone tip is 60°. The structure of this example can increase the breakdown voltage of the device, improve the surface electric field of the GaN HEMT device, reduce the average electric field distribution between the gate and drain, and make the surface electric field distribution of the device more uniform and the withstand voltage capability stronger.
[0096] Example 6
[0097] A groove MIS structure transistor with a toothed p-GaN buried layer comprises a substrate 1, a nucleation layer 2, a first GaN buffer layer 3, a source-drain p-GaN buried layer 4, a second GaN buffer layer 5, a GaN layer 6 and an AlGaN barrier layer 7 which are sequentially arranged from bottom to top; a drain electrode 13 and a source electrode 12 are respectively arranged on both sides of the AlGaN barrier layer 7, a gate electrode groove 8 is arranged on the side of the AlGaN barrier layer 7 close to the drain electrode 13, and a p-GaN layer 9, a gate dielectric layer 10 and a gate electrode 11 which are arranged from bottom to top are arranged in the gate electrode groove 8; toothed protrusions and grooves matching the protrusions are distributed on the opposite sides of the first GaN buffer layer 3 and the second GaN buffer layer 5, the source-drain p-GaN buried layer 4 is located between the first GaN buffer layer 3 and the second GaN buffer layer 5, and the shape of the contact surface between the source-drain p-GaN buried layer 4 and the first GaN buffer layer 3 and the second GaN buffer layer 5 is matched.
[0098] The tooth-like protrusions and grooves on the opposite surfaces of the first GaN buffer layer 3 and the second GaN buffer layer 5 are in a stepped shape; the thickness of the p-GaN buried layer 4 between the source and the drain is 200 nm.
[0099] The first GaN buffer layer 3 is 5 μm thick, the p-GaN buried layer 4 between the source and drain is 200 nm thick, the second GaN buffer layer 5 is 45 μm thick, the GaN layer 6 is 100 nm thick, the AlGaN barrier layer 7 is 60 nm thick, the p-GaN layer 9 is 120 nm thick, and the gate dielectric layer 10 is 20 nm thick.
[0100] The step inclination angle of the stepped shape is 45°.
[0101] The gate electrode 11 is a Schottky contact, the source electrode 12 and the drain electrode 13 are in contact with the AlGaN barrier layer 7 respectively, and the source electrode 12 and the drain electrode 13 are not connected to each other.
[0102] The source electrode 12 and the drain electrode 13 are both made of Ti as the base metal, and are formed by the overall solidification of Ti, Al, Ni and Au from bottom to top. Among them, Ti metal is the barrier layer metal, and Ti diffuses into the AlGaN barrier layer 7 to form TiN with low work function and generate a large number of nitrogen vacancies, thereby forming an ohmic contact. The thicknesses of Ti, Al, Ni and Au are 40nm, 80nm, 40nm and 120nm respectively. Metal Al is the cover layer metal and acts as a catalyst to promote Ti and the nitrogen element in GaN to form TiN; Ni and Au belong to the cap layer metal. Ni prevents the upper layer Au from diffusing downward, and Au plays a protective role to prevent the metal below from being oxidized.
[0103] The gate electrode groove 8 has a depth of 25 nm.
[0104] The p-type doping concentration of the p-GaN buried layer 4 between the source and drain is 8e 17 cm -3 ; The p-type doping concentration in the p-GaN layer 9 is 7e 17 cm -3 .
[0105] The nucleation layer 2 is composed of AlGaN with a gradient Al component, and the Al 0.2 Ga 0.8 N, 200nm thick Al 0.5 Ga 0.5 N and 200nm thick Al 0.8 Ga 0.2 N; the nucleation layer can minimize the lattice mismatch and stress problems in the material epitaxial process, which is beneficial to controlling the quality and stress of the GaN epitaxial layer.
[0106] The gate electrode 11 is 3.5 μm long, the distance between the source electrode and the drain electrode is 15 μm, the distance between the gate electrode and the source electrode is 2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm.
[0107] The gate dielectric layer 10 is made of AlN.
[0108] like Figure 7 As shown, the difference between this example and Example 1 is that the p-GaN buried layer 4 between the source and drain described in this example is a stepped structure between the gate and source, the lateral distance between each small piece of p-GaN is 1μm, and the step inclination angle is 45°. The stepped p-GaN buried layer between the gate and source in this embodiment improves the electric field distribution at the source end of the gate electrode, and the electric field distribution at the drain end of the gate electrode tends to be uniform, close to the critical breakdown electric field, thereby improving the breakdown voltage of the device and reducing the leakage of the gate electrode.
[0109] like Figure 8As shown in the figure, the breakdown characteristics of the present invention and the traditional device are compared. Among them, the traditional device refers to the conventional p-GaN HEMT device without the p-GaN buried layer. It can be seen that the conventional p-GaN HEMT device will break down at about 400V, which limits the application of the device in high-voltage scenarios. The transistor of the present invention sets a toothed source-drain p-GaN buried layer in the GaN buffer layer, which improves the overall electric field distribution of the device, has a better electric field relief effect, can improve the breakdown voltage of the device, and the breakdown voltage exceeds 1400V, which improves the reliability of the device and can be applied to high-voltage and high-power application scenarios.
[0110] The above are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A groove MIS structure transistor with a toothed p-GaN buried layer, comprising a substrate (1), a nucleation layer (2), a first GaN buffer layer (3), a source-drain p-GaN buried layer (4), a second GaN buffer layer (5), a GaN layer (6) and an AlGaN barrier layer (7) arranged in sequence from bottom to top; It is characterized in that A drain electrode (13) and a source electrode (12) are respectively arranged on both sides of the AlGaN barrier layer (7); a gate electrode groove (8) is arranged on one side of the AlGaN barrier layer (7) close to the drain electrode (13); a p-GaN layer (9), a gate dielectric layer (10) and a gate electrode (11) are arranged from bottom to top in the gate electrode groove (8); tooth-shaped protrusions and grooves matching the protrusions are distributed on the opposite sides of the first GaN buffer layer (3) and the second GaN buffer layer (5); a source-drain p-GaN buried layer (4) is located between the first GaN buffer layer (3) and the second GaN buffer layer (5); and the shape of the contact surface between the source-drain p-GaN buried layer (4) and the first GaN buffer layer (3) and the second GaN buffer layer (5) is matched.
2. A groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1, It is characterized in that The tooth-shaped protrusions and grooves on the opposite surfaces of the first GaN buffer layer (3) and the second GaN buffer layer (5) are square, arc-shaped, conical, trapezoidal or stepped; the thickness of the p-GaN buried layer (4) between the source and the drain is 150nm to 300nm.
3. A groove MIS structure transistor with a toothed p-GaN buried layer according to claim 2, It is characterized in that The cone tip angle of the cone is 30° to 60°, the inclination angle of the trapezoid is 45° to 90°, and the step inclination angle of the step shape is 45° to 60°.
4. The groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1, It is characterized in that The gate electrode (11) is a Schottky contact, the source electrode (12) and the drain electrode (13) are in contact with the AlGaN barrier layer (7) respectively, and the source electrode (12) and the drain electrode (13) are not connected to each other.
5. A groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1 or 4, It is characterized in that The source electrode (12) and the drain electrode (13) both use Ti as a base metal, and are formed by integrally solidifying Ti, Al, Ni and Au from bottom to top, wherein Ti metal is a barrier layer metal, and Ti diffuses into the AlGaN barrier layer (7) to form TiN with a low work function and generate nitrogen vacancies, thereby forming an ohmic contact.
6. The groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1, It is characterized in that The gate electrode groove (8) has a depth of 20 nm to 25 nm.
7. The groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1, It is characterized in that The p-type doping concentration of the p-GaN buried layer (4) between the source and drain is 3e 16 cm -3 ~8e 17 cm -3 ; The p-type doping concentration in the p-GaN layer (9) is 5e 17 cm -3 ~7e 17 cm -3 .
8. The groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1, It is characterized in that The nucleation layer (2) is composed of AlGaN with a gradient Al component, and the thickness of Al from bottom to top is 150nm to 200nm. 0.2 Ga 0.8 N, 150nm~200nm thick Al 0.5 Ga 0.5 N and 150nm~200nm thick Al 0.8 Ga 0.2 N.
9. The groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1, It is characterized in that The gate electrode (11) is 3.5-4.0 μm long, the distance between the source electrode and the drain electrode is 10-15 μm, the distance between the gate electrode and the source electrode is 1-2.5 μm, and the distance between the gate electrode and the drain electrode is 8.5 μm-10 μm.
10. The groove MIS structure transistor with a toothed p-GaN buried layer according to claim 1, It is characterized in that The gate dielectric layer (10) is made of a high dielectric constant dielectric material, including Al 2 O 3 、AlN。
Citation Information
Patent Citations
Semiconductor device and manufacturing method thereof
CN112018176A
Homoepitaxial gallium nitride high-electron-mobility transistor based on P-type GaN electric leakage isolation layer and manufacturing method of homoepitaxial gallium nitride high-electron-mobility transistor
CN113555431A
Single-particle-resistant P-GaN transistor with buried layer structure and preparation method of single-particle-resistant P-GaN transistor
CN116913960A
Field effect semiconductor device and its fabrication process
JP2008210836A
Cited By
Nitride enhanced field effect transistor based on P buried layer
CN119947166A