Composite current collector, battery and preparation method of composite current collector
By loading MOF plating on the surface of the composite fluid-collection metal plating layer to form a three-dimensional metal organic framework, the battery short circuit and thermal runaway caused by lithium dendrites piercing the diaphragm is solved, and more stable battery performance and longer battery life are achieved.
Patent Information
- Application Number
- CN202411185342.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-27
AI Technical Summary
During the charge and discharge cycle of composite liquid collecting, the large amount of lithium dendrites will pierce the diaphragm, resulting in battery short circuit and thermal runaway.
A MOF coating is loaded on the surface of the metal plating layer of the composite fluid, and the MOF is loaded by magnetron sputtering to form a three-dimensional, high-strength metal organic framework, inhibit the growth of lithium dendrites, and improve the electrodes through metal atoms and nitrogen atoms. lithium plating process.
It effectively inhibits the formation of lithium dendrites, improves the cycling stability and ionic conductivity of the battery, reduces the local current density, extends the battery life and improves the battery performance.
Smart Images

Figure CN118919732A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite current collectors, in particular to a composite current collector, a battery and a method for preparing the composite current collector. Background Art
[0002] The battery current collector is an important component of the battery. It is connected to the positive and negative electrodes of the battery. Its main function is to concentrate the current inside the battery so that the battery can output more stable and efficient electricity. Traditional current collectors are usually made of metals with good conductivity such as copper and silver. Large-sized burrs are easily generated during the production process, causing internal short circuits and thermal runaway. Now, composite current collectors are more likely to be used. Composite current collectors use raw material films such as PET as base films and are deposited on both sides with copper or aluminum composite materials through processes such as magnetron sputtering or vacuum coating to form a "metal-polymer material-metal" three-layer composite structure. Because of its high stability and conductivity, it is widely used as a current collector material for lithium-ion batteries.
[0003] Although the burrs produced by the composite current collector are small in size, the short-circuit effect caused by the superimposed polymer material layer being heated can greatly reduce the short-circuit current in a short period of time, but as the charge and discharge cycle proceeds, the inherent protrusions on the current collector surface will cause excessive Li ion flow, eventually forming a local uneven current density. A large number of lithium dendrites will form on the current collector surface, and the large number of lithium dendrites will pierce the diaphragm, resulting in short circuit and thermal runaway of the battery. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a composite current collector, a battery and a method for preparing the composite current collector. The MOF coating on the composite current collector can effectively inhibit the growth of lithium dendrites, thereby solving the problem that a large number of lithium dendrites will pierce the diaphragm, thereby causing short circuit and thermal runaway of the battery.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] In a first aspect, a composite current collector includes a polymer macromolecular base layer, metal coatings are provided on both sides of the polymer macromolecular base layer, and a MOF coating is provided on a side of the metal coating layer away from the polymer macromolecular base layer.
[0007] As a further implementation, the material of the metal plating layer is selected from copper or aluminum.
[0008] As a further implementation method, the MOF coating is loaded on the surface of the metal coating by magnetron sputtering.
[0009] As a further implementation method, the total thickness of the polymer base layer, metal coating and MOF coating is between 1.5 μm and 4.5 μm.
[0010] As a further implementation, the material of the polymer macromolecular base layer is selected from one or more of polyethylene, polypropylene, and thermoplastic polyester.
[0011] As a further implementation, the material of the MOF coating is selected from 2-methylimidazole solution and nitrate solution.
[0012] In a second aspect, a method for preparing a composite current collector comprises the following steps:
[0013] A metal coating is deposited on the upper and lower surfaces of a polymer macromolecular base layer; a 2-methylimidazole solution and a nitrate solution are mixed in a set ratio to obtain a mixed solution, the mixed solution is heated and dried, and then calcined under the protection of nitrogen to synthesize a MOF coating; the prepared MOF coating is loaded on the outer surface of the metal coating by magnetron sputtering to obtain any of the composite current collectors described above.
[0014] As a further implementation, the concentration ratio of the 2-methylimidazole solution to the nitrate solution is in the range of 10:1-5:1.
[0015] As a further implementation, the heating temperature of the mixed solution is 110° C.-130° C., and the heating time is 8-10 hours; the flow rate of the nitrogen is 5° C. / min.
[0016] A third aspect provides a battery, comprising any composite current collector as described above.
[0017] The beneficial effects of the present invention are as follows:
[0018] The present invention loads a layer of MOF coating on the metal coating surface of the original composite current collector to obtain an improved composite current collector, which is enhanced by a three-dimensional, high-strength, interconnected MOF network. Based on its 3D skeleton, the mobility of electrons can be improved. Thereby forming an ultrafast ion transport network with excellent ionic conductivity. Secondly, the metal atoms and N atoms loaded on the MOF can effectively convert the lithium-phobicity of the carbon material into lithium-philicity, thereby promoting the lithium plating process on the electrode. Furthermore, by reducing the local current density and limiting the volume change in the three-dimensional network porous structure, the growth of dendrites can be effectively suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0020] Figure 1 Schematic diagram of the structure of the composite current collector in an embodiment of the present invention.
[0021] In the figure: the distances or sizes between parts are exaggerated to show the positions of various parts, and the schematic diagram is for reference only.
[0022] Among them: 1: MOF coating, 2: metal coating, 3: polymer base layer. DETAILED DESCRIPTION
[0023] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0024] Embodiment 1
[0025] In a typical embodiment of the present invention, reference is made to Figure 1 As shown, a composite current collector comprises a polymer macromolecular base layer 3, a metal coating layer 2 and a MOF coating layer 1, wherein the metal coating layer 2 is coated on the upper and lower surfaces of the polymer macromolecular base layer 3, and the MOF coating layer 1 is disposed on the outer surface of the metal coating layer 2. The total thickness of the composite current collector is between 1.5 μm and 4.5 μm.
[0026] Specifically, the polymer high molecular base layer 3 and the metal coating 2 form a three-layer composite structure of "metal-polymer material-metal", which is a prior art. The material of the metal coating 2 is selected from copper or aluminum. The polymer high molecular base layer 3 can be PET, PP, PE, etc. PE is polyethylene, PP is polypropylene, and PET is commonly known as polyester resin. It is a condensation product of terephthalic acid and ethylene glycol, and is collectively referred to as thermoplastic polyester or saturated polyester together with PBT. The metal coating 2 is loaded on the polymer high molecular base layer 3 by processes such as magnetron sputtering or vacuum coating.
[0027] The MOF coating 1 is a metal organic framework. In order to control the uniform deposition of lithium ions, the surface of the existing composite current collector is modified in this embodiment to achieve the purpose of uniform distribution of current density, improved cycle stability and prevention of lithium dendrites. Among them, the metal organic framework (MOF) is a new type of crystalline porous material that self-assembles transition metal ions and organic ligands to form a periodic network structure.
[0028] MOF has the characteristics of high porosity, low density, regular pores, and adjustable pore size, and has obvious advantages in high-performance three-dimensional current collectors. At the same time, the metal atoms and nitrogen atoms produced by MOF during the carbonization process can effectively convert the lithium-phobicity of carbon materials into lithium-philicity, thereby promoting the lithium plating process on the electrode. In addition, by reducing the local current density and limiting the volume change within the three-dimensional network porous structure, the growth of dendrites can be effectively inhibited. This also enables this layered host to adapt to the precipitation of lithium with high area load, while greatly reducing the formation of lithium dendrites, and lithium dendrites are mostly precipitated in a planar two-dimensional form, solving the problem that the large-scale generation of lithium dendrites will pierce the diaphragm, thereby causing short circuit and thermal runaway of the battery.
[0029] Embodiment 2
[0030] In a typical embodiment of the present invention, reference is made to Figure 1 As shown, a method for preparing a composite current collector includes first depositing a metal coating 2 on the upper and lower surfaces of a polymer macromolecular base layer 3 , then preparing MOF, and loading the prepared MOF on the surface of the metal coating 2 .
[0031] The preparation steps of MOF are as follows: a 2-methylimidazole solution and a nitrate solution are mixed to obtain a mixed solution, wherein the concentration ratio of the amount of 2-methylimidazole substance to the amount of nitrate solution substance is in the range of 10:1 to 5:1.
[0032] The mixed solution was heated at 110°C to 130°C for 8 to 10 hours, centrifuged and dried, and then calcined at 400°C to 500°C under the protection of N2 at a flow rate of 5°C / min to synthesize MOF.
[0033] The prepared MOF is loaded on the surface of the metal coating layer 2 by magnetron sputtering or hydrothermal evaporation to form a composite current collector with the surface loaded with the MOF coating layer 1, with a thickness of 1.5 to 5 μm.
[0034] Implementation method 1:
[0035] A metal coating 2 is provided on the upper and lower surfaces of the polymer macromolecular base layer 3 by magnetron sputtering, and a 0.5 mol / L 2-methylimidazole solution and a 0.05 mol / L cobalt nitrate solution are mixed. The mixed solution is heated at 110°C for 8 hours and centrifugally dried. Thereafter, MOF is synthesized by calcination at 400°C under the protection of N2 at a flow rate of 5°C / min. The prepared MOF is loaded on the surface of the metal coating by magnetron sputtering to form a composite current collector with a surface loaded MOF and a thickness of 1.5 μm.
[0036] Implementation method 2:
[0037] A metal coating 2 is provided on the upper and lower surfaces of the polymer macromolecular base layer 3 by magnetron sputtering, and a 0.25 mol / L 2-methylimidazole solution and a 0.05 mol / L cobalt nitrate solution are mixed. The mixed solution is heated at 110°C for 8 hours and centrifugally dried. Then, under the protection of N2 at a flow rate of 5°C / min, MOF is synthesized by calcination at 400°C. The prepared MOF is loaded on the surface of the metal coating 2 by magnetron sputtering or hydrothermal evaporation to form a composite current collector with a surface loaded MOF coating 1 having a thickness of 1.5 μm.
[0038] Implementation Method 3
[0039] A metal coating 2 is provided on the upper and lower surfaces of the polymer macromolecular base layer 3 by magnetron sputtering, and a 0.5 mol / L 2-methylimidazole solution and a 0.05 mol / L cobalt nitrate solution are mixed; the mixed solution is heated at 110°C for 8 hours and centrifugally dried. Then, under the protection of N2 at a flow rate of 5°C / min, MOF is synthesized by calcination at 400°C. The prepared MOF is loaded on the surface of the metal coating 2 by magnetron sputtering or hydrothermal evaporation to form a composite current collector with a surface loaded MOF coating 1, and the thickness is 4.5 μm.
[0040] Implementation Method 4
[0041] A metal coating 2 is provided on the upper and lower surfaces of the polymer macromolecular base layer 3 by magnetron sputtering, and a 0.5 mol / L 2-methylimidazole solution and a 0.05 mol / L zinc nitrate solution are mixed; the mixed solution is heated at 110°C for 10 hours and centrifugally dried. Then, under the protection of N2 at a flow rate of 5°C / min, MOF is synthesized by calcination at 400°C. The prepared MOF is loaded on the surface of the metal coating 2 by magnetron sputtering or hydrothermal evaporation to form a composite current collector with a surface loaded MOF coating 1, and the thickness is 1.5 μm.
[0042] Implementation Method 5
[0043] A metal coating 2 is provided on the upper and lower surfaces of the polymer macromolecular base layer 3 by magnetron sputtering, and a 0.5 mol / L 2-methylimidazole solution and a 0.05 mol / L zinc nitrate solution are mixed; the mixed solution is heated at 130°C for 10 hours and centrifugally dried. Then, under the protection of N2 at a flow rate of 5°C / min, MOF is synthesized by calcination at 500°C. The prepared MOF is loaded on the surface of the metal coating 2 by magnetron sputtering or hydrothermal evaporation to form a composite current collector with a surface loaded MOF coating 1, and the thickness is 1.5 μm.
[0044] Comparative Example 1:
[0045] The difference from the above-mentioned embodiment 1 is that: no 2-methylimidazole solution is used, and only cobalt nitrate solution is used.
[0046] Comparative Example 2:
[0047] The difference from the above-mentioned embodiment 1 is that a blank composite current collector is used, that is, the MOF coating is not loaded on the surface of the composite current collector.
[0048] Table 1
[0049]
[0050]
[0051] Table 1 above is a comparison of the performance of materials in different implementations and comparative examples. It can be concluded that the composite current collector with a MOF coating 1 on the surface finally forms only a small amount of lithium dendrites on the current collector surface, while in the comparative example, the MOF in comparative example 1 uses a cobalt nitrate solution alone, and comparative example 2 does not load a MOF coating, and finally forms more lithium dendrites on the current collector surface. In addition, the three indicators of tensile strength, elongation and cycle capacity retention rate of the comparative example are all weaker than those of implementation examples 1 to 5.
[0052] The present embodiment proposes to prepare a metal organic framework MOF, and load the prepared MOF on the surface of the metal coating 2 of the original composite current collector by magnetron sputtering, so as to obtain a composite current collector that can prevent lithium dendrites and improve cycle stability. This composite current collector is enhanced by a three-dimensional, high-strength, interconnected MOF network. Based on its 3D skeleton, the mobility of electrons can be improved. Thereby forming an ultrafast ion transport network with excellent ionic conductivity. Secondly, the metal atoms and N atoms loaded on the MOF can effectively convert the lithium-phobicity of the carbon material into lithium-philicity, thereby promoting the lithium plating process on the electrode. Furthermore, by reducing the local current density and limiting the volume change in the three-dimensional network porous structure, the growth of dendrites can be effectively suppressed.
[0053] Embodiment 3
[0054] In a typical embodiment of the present invention, a battery includes a composite current collector as in Example 1, and only a small amount of lithium dendrites will be formed on the composite current collector in the battery, thereby increasing the battery life and improving the battery performance.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite current collector, characterized in that: The invention comprises a polymer macromolecular base layer, two side surfaces of the polymer macromolecular base layer are provided with metal coatings, and a side of the metal coating layer away from the polymer macromolecular base layer is provided with an MOF coating.
2. A composite current collector according to claim 1, characterized in that: The material of the metal plating layer is selected from copper or aluminum.
3. A composite current collector according to claim 1, characterized in that: The MOF coating is loaded on the surface of the metal coating by magnetron sputtering.
4. A composite current collector according to claim 1, characterized in that: The total thickness of the polymer base layer, the metal coating layer and the MOF coating layer is between 1.5 μm and 4.5 μm.
5. A composite current collector according to claim 1, characterized in that: The material of the polymer macromolecular base layer is selected from one or more of polyethylene, polypropylene, and thermoplastic polyester.
6. A composite current collector according to claim 1, characterized in that: The material of the MOF coating is selected from 2-methylimidazole solution and nitrate solution.
7. A method for preparing a composite current collector, characterized in that: The steps include: Depositing metal coatings on the upper and lower surfaces of the polymer macromolecular base layer; A 2-methylimidazole solution and a nitrate solution are mixed in a set ratio to obtain a mixed solution, the mixed solution is heated and dried, and then calcined under the protection of nitrogen to synthesize a MOF coating; the prepared MOF coating is loaded on the outer surface of the metal coating by magnetron sputtering to obtain a composite current collector as described in any one of claims 1 to 6.
8. The method for preparing a composite current collector according to claim 7, characterized in that: The concentration ratio of the 2-methylimidazole solution to the nitrate solution is in the range of 10:1-5:
1.
9. The method for preparing a composite current collector according to claim 7, characterized in that: The heating temperature of the mixed solution is 110° C.-130° C., and the heating time is 8-10 hours; the flow rate of the nitrogen is 5° C. / min.
10. A battery, characterized in that: A battery comprises the composite current collector as claimed in any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method and application of low-volume-change metal secondary battery negative electrode
CN109980235A
Negative current collector, preparation method thereof, negative pole piece with negative current collector, and lithium secondary battery
CN115842133A
Composite current collector, preparation method thereof and application of composite current collector in negative-electrode-free lithium metal battery
CN118099440A
Negative electrode plate and preparation method therefor, secondary battery, battery module, battery pack and power consuming devic
US20240194889A1
KR20220128947A