Recycling method of lithium ion battery

Through the combination of nitric acid leaching, hydrogenation and carbonation, combined with magnetic separation and water dissolution steps, the problems of poor selectivity and environmental pollution in lithium-ion battery recycling are solved, the recovery rate and separation effect are improved, and acid-free Wastewater treatment.

CN118919909APending Publication Date: 2024-11-08SI CHUAN ZHI HUI XIN NENG YUAN YOU XIAN GONG SI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411081423.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing lithium-ion battery recycling technology has problems such as poor selectivity, low recovery rate and serious environmental pollution, especially the pyrometallurgy and hydrometallurgy processes have their own shortcomings in the metal element extraction process.

Method used

By combining nitric acid leaching, hydrogenation and carbonation, lithium carbonate solution and metal carbonate are separated by mixing and disassembling the positive electrode powder, catalyst and nitric acid react under heating conditions, combining magnetic separation and water dissolution steps, lithium carbonate solution and metal carbonate are separated. Avoid the generation of acidic wastewater and pollutants.

Benefits of technology

The process flow is simplified, the separation effect and recovery rate of metal elements are improved, environmental pollution is reduced, and the generation of acid-free wastewater is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919909A_ABST
    Figure CN118919909A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of resource recovery, and discloses a lithium ion battery recovery method which comprises the following steps: step 1, mixing and disassembling positive electrode powder, a catalyst and nitric acid to react under a heating condition, and introducing hydrogen and carbon dioxide into a reaction system at the same time; after the reaction, carrying out solid-liquid separation to obtain an ammonium bicarbonate solution and leaching residues; 2, the leaching residues are subjected to magnetic separation, and a catalyst and magnetic separation residues are obtained; and step 3, dissolving the magnetic separation slag with water, and then carrying out solid-liquid separation to obtain a lithium carbonate solution and metal carbonate. According to the method, recycling of the waste lithium ion battery is achieved through combination of nitric acid leaching, hydrogenation ammonia preparation and carbonation, and compared with a traditional wet metallurgy process, the process is simplified, and no acid waste water or other pollutants are generated; and the separation effect of metal elements can be improved, and the recovery rate is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of resource recovery, and relates to the recovery of lithium battery related materials, and specifically to a method for recovering lithium ion batteries. Background Art

[0002] Lithium-ion batteries contain a large amount of toxic and hazardous substances and heavy metals, so it is not feasible to simply landfill them. Considering the protection of the environment and the recycling of resources, the recycling of used lithium-ion batteries has become an essential part of the development of the new energy industry.

[0003] In the prior art, various metal elements in waste lithium-ion batteries are usually recovered through pyrometallurgy and hydrometallurgy. Pyrometallurgy has great advantages in adaptability and flexibility, but its selectivity for metal elements is poor, the recovery rate is low, and it seriously pollutes the environment. Hydrometallurgy has strong selectivity for metal elements and high recovery rate, but it needs to use a variety of acid solutions and other solvents for extraction, resulting in large amounts of wastewater and complex subsequent treatment. Summary of the invention

[0004] In view of the defects and shortcomings of the prior art, the present invention provides a method for recycling lithium ion batteries.

[0005] The present invention provides a method for recycling lithium ion batteries, comprising the following steps: Step 1, mixing and disassembling the cathode powder, the catalyst and nitric acid to react under heating conditions, while introducing hydrogen and carbon dioxide into the reaction system; after the reaction, the solid and liquid are separated to obtain an ammonium bicarbonate solution and leaching residue; Step 2, magnetically separating the leached residue to obtain a catalyst and magnetically separated residue; Step 3, using water to dissolve the magnetic separation slag and then separate the solid and liquid to obtain lithium carbonate solution and metal carbonate.

[0006] Preferably, the catalyst consists of a magnetic substance and a transition metal.

[0007] More preferably, the magnetic material is any one or more of iron, cobalt and nickel; and the transition metal is any one or more of ruthenium, rhodium and palladium.

[0008] More preferably, in the catalyst, the mass ratio of the magnetic substance to the transition metal is 1:1 to 5:1.

[0009] Preferably, the positive electrode powder is any one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and lithium nickel cobalt manganese oxide.

[0010] Preferably, in step 1, the amount of catalyst added is 5% to 20% of the mass of the positive electrode powder; the solid-liquid ratio of the positive electrode powder to nitric acid is 5 to 50 g / L; and the concentration of nitric acid is 0.5 to 3 mol / L.

[0011] Preferably, in step 1, during the reaction process, the molar ratio of hydrogen to carbon dioxide in the reaction system is controlled to be 1-2.5:1.

[0012] Preferably, in step 1, the pressure in the reaction system is 0.5-5 MPa; the reaction temperature is 80-120° C.; and the reaction time is 1-12 h.

[0013] Preferably, in step 3, the solid-liquid ratio when the magnetic separation slag is dissolved in water is 1-10 g / L.

[0014] Preferably, in step 3, the time for dissolving the magnetic separation slag with water is 5 to 60 minutes.

[0015] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects: This method utilizes a combination of nitric acid leaching, hydrogenation to produce ammonia and carbonation to recycle waste lithium-ion batteries. Compared with traditional hydrometallurgical processes, it not only simplifies the process, but also does not produce acidic wastewater and other pollutants; it can also improve the separation effect of metal elements and increase the recovery rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A schematic diagram of the process of the lithium ion battery recycling method provided by the present invention. DETAILED DESCRIPTION

[0017] The present invention provides the following specific technical solutions.

[0018] In a first aspect, the present invention provides a method for recycling a lithium battery, comprising the following steps: Step 1, mixing the disassembled cathode powder, catalyst and nitric acid, reacting them at a certain pressure and temperature, while introducing hydrogen and carbon dioxide; after reacting for a certain period of time, solid-liquid separation is performed to obtain ammonium bicarbonate solution and leaching residue; Step 2, magnetically separating the leached residue to obtain a catalyst and magnetically separated residue; Step 3, using water to dissolve the magnetic separation slag and then separate the solid and liquid to obtain lithium carbonate solution and metal carbonate.

[0019] Preferably, the catalyst consists of a magnetic substance and a transition metal.

[0020] More preferably, the magnetic material is any one or more of iron, cobalt and nickel; and the transition metal is any one or more of ruthenium, rhodium and palladium.

[0021] In the present invention, magnetic material and transition metal are combined, so that the catalyst can be separated from the solid phase by magnetic separation after the reaction is completed. In practical applications, the preparation method disclosed in patent CN110624609A can be referred to to prepare the catalyst by combining magnetic material and transition metal with a binder.

[0022] More preferably, the mass ratio of the magnetic substance to the transition metal is 1:1 to 5:1.

[0023] In actual production, the ratio of magnetic substance to transition metal can be adjusted according to the actual situation. If there is too much magnetic substance or too little transition metal, the effective contact area between reactants and transition metal will be reduced, resulting in reduced catalytic efficiency; if there is too little magnetic substance or too much transition metal, the separation effect between catalyst and product will be reduced, and the purity of the product will be reduced. Therefore, the inventors propose a preferred range: the mass ratio of magnetic substance to transition metal is 1:1~5:1.

[0024] Preferably, the positive electrode powder is any one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and lithium nickel cobalt manganese oxide.

[0025] Preferably, in step 1, the mass of the added catalyst is 5% to 20% of the positive electrode powder; the solid-liquid ratio of the positive electrode powder to nitric acid is 5 to 50 g / L; and the concentration of nitric acid is 0.5 to 3 mol / L.

[0026] In actual production, the amount of catalyst and nitric acid added can be adjusted according to the actual situation. If the amount of catalyst added is too much or the amount of nitric acid added is too little, a large amount of nitric acid will be consumed during the reaction, resulting in a decrease in the leaching rate of the positive electrode powder; if the amount of catalyst added is too little or the amount of nitric acid added is too much, the nitrate ions in the solution cannot be completely converted, thereby generating waste acid. Therefore, the inventors propose the above preferred range.

[0027] Preferably, in step 1, during the reaction process, the molar ratio of hydrogen to carbon dioxide in the reaction system is controlled to be 1-2.5:1.

[0028] Preferably, in step 1, the pressure in the reaction system is 0.5-5 MPa; the reaction temperature is 80-120° C.; and the reaction time is 1-12 h.

[0029] In actual production, if the pressure or temperature in the reaction system is too high, the activity of the catalyst may be reduced, thereby causing a decrease in the catalytic reaction rate; if the pressure or temperature in the reaction system is too low, the reaction rate of the leaching process will be reduced, thereby reducing production efficiency.

[0030] Preferably, in step 3, the solid-liquid ratio when the magnetic separation slag is dissolved in water is 1-10 g / L.

[0031] Preferably, in step 3, the time for dissolving the magnetic separation slag with water is 5 to 60 minutes.

[0032] In order to make the technical problems, technical solutions and technical advantages to be solved by the present invention more clear, they will be described in detail below with reference to specific examples, but the protection scope of the present invention is not limited to the following specific embodiments.

[0033] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0035] Embodiment 1: A lithium battery recycling method comprises the following steps: Step 1: dismantle the cathode plate of the waste lithium battery, crush it, and obtain cathode powder. The magnetic material and transition metal of the catalyst are iron and ruthenium, respectively, with a mass ratio of 3:1.

[0036] Step 2: Take 10g of positive electrode powder, 1.2g of catalyst and 350ml of 2mol / L nitric acid, mix them evenly and add them into a high-pressure reactor to react for 6h. The temperature of the reaction system is 100°C. At the same time, hydrogen and carbon dioxide are introduced into the reaction system. The molar ratio of hydrogen and carbon dioxide in the reaction system is controlled to be 3:1, and the pressure of the reaction system is maintained at about 3MPa.

[0037] Step 3, after the reaction is completed, the slurry in the high-pressure reactor is solid-liquid separated to obtain an ammonium bicarbonate solution and leached residue.

[0038] Step 4, magnetically separating the leached residue to separate the catalyst in the leached residue to obtain magnetically separated residue.

[0039] Step 5, dissolve 5 g of magnetic separation slag in 1 L of water, stir for 30 min, and separate the solid and liquid to obtain lithium carbonate solution and metal carbonate.

[0040] The ammonium bicarbonate solution obtained in step 3 was detected by spectrophotometry, and no nitrate ions were detected therein.

[0041] The contents of lithium in the lithium carbonate solution obtained in step 5 and nickel, cobalt and manganese in the metal carbonate were determined by inductively coupled plasma emission spectrometry. The recovery rate of lithium was 98.7%, and the comprehensive recovery rate of nickel, cobalt and manganese was 98.9%.

[0042] Embodiment 2: A lithium battery recycling method comprises the following steps: Step 1: dismantle the cathode sheet of the waste lithium battery, crush it, and obtain cathode powder. The magnetic material and transition metal of the catalyst are cobalt and rhodium, respectively, and the mass ratio thereof is 1:1.

[0043] Step 2: 100 g of positive electrode powder, 5 g of catalyst and 20 L of 0.5 mol / L nitric acid were mixed evenly and added to a high-pressure reactor for reaction for 1 h, and the temperature of the reaction system was 80° C. Hydrogen and carbon dioxide were introduced at the same time, and the molar ratio of hydrogen and carbon dioxide in the reaction system was controlled to be 1:1, and the pressure of the reaction system was maintained at about 0.5 MPa.

[0044] Step 3, after the reaction is completed, the slurry in the high-pressure reactor is solid-liquid separated to obtain an ammonium bicarbonate solution and leached residue.

[0045] Step 4, magnetically separating the leached residue to separate the catalyst in the leached residue to obtain magnetically separated residue.

[0046] Step 5, use 10L of water to dissolve 10g of magnetic separation slag, stir for 10min and separate the solid and liquid to obtain lithium carbonate solution and metal carbonate.

[0047] The ammonium bicarbonate solution obtained in step 3 was detected by spectrophotometry, and no nitrate ions were detected therein.

[0048] The contents of lithium in the lithium carbonate solution obtained in step 5 and nickel, cobalt and manganese in the metal carbonate were determined by inductively coupled plasma emission spectrometry. The recovery rate of lithium was 96.6%, and the comprehensive recovery rate of nickel, cobalt and manganese was 96.9%.

[0049] Embodiment 3: A lithium battery recycling method comprises the following steps: Step 1: dismantle the cathode plate of the waste lithium battery, crush it, and obtain cathode powder. The magnetic material and transition metal of the catalyst are nickel and palladium, respectively, with a mass ratio of 5:1.

[0050] Step 2: 10 g of positive electrode powder, 2 g of catalyst and 200 mL of 3 mol / L nitric acid were mixed evenly and added into a high-pressure reactor for reaction for 12 h, and the temperature of the reaction system was 120° C. Hydrogen and carbon dioxide were introduced at the same time, and the molar ratio of hydrogen to carbon dioxide in the reaction system was controlled to be 5:1, and the pressure of the reaction system was maintained at about 5 MPa.

[0051] Step 3, after the reaction is completed, the slurry in the high-pressure reactor is solid-liquid separated to obtain an ammonium bicarbonate solution and leached residue.

[0052] Step 4, magnetically separating the leached residue to separate the catalyst in the leached residue to obtain magnetically separated residue.

[0053] Step 5, using 500 mL of water to dissolve 5 g of magnetic separation slag, stirring for 60 min and then separating the solid and liquid to obtain lithium carbonate solution and metal carbonate.

[0054] The ammonium bicarbonate solution obtained in step 3 was detected by spectrophotometry, and no nitrate ions were detected therein.

[0055] The contents of lithium in the lithium carbonate solution obtained in step 5 and nickel, cobalt and manganese in the metal carbonate were determined by inductively coupled plasma emission spectrometry. The recovery rates of lithium and nickel, cobalt and manganese were calculated to be 99.3%, and 99.1%.

[0056] Comparative Example 1: A lithium battery recycling method comprises the following steps: Step 1: dismantle the cathode sheet of the waste lithium battery, crush it, and obtain cathode powder. The magnetic material and transition metal of the catalyst are nickel and palladium, respectively, and the mass ratio thereof is 3:1.

[0057] Step 2: 10 g of positive electrode powder, 1.2 g of catalyst and 350 ml of 2 mol / L nitric acid were mixed evenly and added into a high-pressure reactor for reaction for 6 h. The temperature of the reaction system was 100° C. Carbon dioxide was introduced at the same time, but hydrogen was not introduced, and the pressure of the reaction system was maintained at about 3 MPa.

[0058] Step 3, after the reaction is completed, the slurry in the high-pressure reactor is solid-liquid separated to obtain a leachate and a leach residue.

[0059] Step 4, magnetically separating the leached residue to separate the catalyst in the leached residue to obtain magnetically separated residue.

[0060] Step 5, dissolve 5 g of magnetic separation slag in 1 L of water, stir for 30 min, and separate the solid and liquid to obtain lithium carbonate solution and metal carbonate.

[0061] The ammonium bicarbonate solution obtained in step 3 is detected by spectrophotometry, and a large amount of nitrate ions are detected in the ammonium bicarbonate solution. By comparing the detection results of the ammonium bicarbonate solutions in Examples 1 to 3, it can be seen that the recovery method provided by the present invention can improve the efficiency of converting nitrate ions in the waste liquid into ammonium ions, without the need to treat the waste liquid.

[0062] The contents of lithium in the lithium carbonate solution obtained in step 5 and nickel, cobalt and manganese in the metal carbonate were determined by inductively coupled plasma emission spectrometry. The recovery rate of lithium was 99.1%, and the comprehensive recovery rate of nickel, cobalt and manganese was 98.9%.

[0063] By analyzing the test data of Examples 1 to 3 and Comparative Example 1, the inventors speculated that the principle of the present invention is: the metal elements in the positive electrode powder are leached using the acidity and strong oxidizing property of nitric acid to generate metal nitrates; at the same time, carbon dioxide enters the solution under a certain pressure to generate carbonate ions, which react with metal ions in the solution to generate water-insoluble metal carbonates, and the mixture composed of lithium carbonate and other metal carbonates is precipitated and separated from the liquid phase, and then separated using the solubility difference of lithium carbonate and metal carbonate at room temperature to obtain lithium carbonate solution and metal carbonate respectively. The nitrate ions in the solution react with hydrogen under the action of a catalyst to be converted into ammonium ions, and the method provided by the present invention can simultaneously achieve the leaching of positive electrode powder and the treatment of waste acid.

[0064] The embodiments described above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and concepts of the present invention within the technical scope of the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for recycling lithium-ion batteries, It is characterized in that The steps include: Step 1, mixing and disassembling the cathode powder, the catalyst and nitric acid to react under heating conditions, while introducing hydrogen and carbon dioxide into the reaction system; after the reaction, the solid and liquid are separated to obtain an ammonium bicarbonate solution and leaching residue; Step 2, magnetically separating the leached residue to obtain a catalyst and magnetically separated residue; Step 3, using water to dissolve the magnetic separation slag and then separate the solid and liquid to obtain a lithium carbonate solution and metal carbonate; Wherein, the catalyst is composed of magnetic material and transition metal.

2. The method for recovering lithium ions according to claim 1, It is characterized in that The positive electrode powder is any one or two or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and lithium nickel cobalt manganese oxide.

3. The method for recovering lithium ions according to claim 1, It is characterized in that The magnetic material is any one or more of iron, cobalt and nickel; the transition metal is any one or more of ruthenium, rhodium and palladium.

4. The method for recovering lithium ions according to claim 1 or 3, It is characterized in that In the catalyst, the mass ratio of the magnetic substance to the transition metal is 1:1 to 5:

1.

5. The method for recovering lithium ions according to claim 1 or 3, It is characterized in that In step 1, the amount of catalyst added is 5% to 20% of the mass of the positive electrode powder; the solid-liquid ratio of the positive electrode powder and nitric acid is 5 to 50 g / L; and the concentration of nitric acid is 0.5 to 3 mol / L.

6. The method for recovering lithium ions according to claim 1, It is characterized in that In step 1, during the reaction process, the molar ratio of hydrogen to carbon dioxide in the reaction system is controlled to be 1-2.5:

1.

7. The method for recovering lithium ions according to claim 1 or 6, It is characterized in that In step 1, the pressure in the reaction system is 0.5~5MPa; the reaction temperature is 80~120°C; and the reaction time is 1~12h.

8. The method for recovering lithium ions according to claim 1, It is characterized in that In step 3, the solid-liquid ratio when water dissolves the magnetic separation slag is 1-10 g / L.

9. The method for recovering lithium ions according to claim 1 or 8, It is characterized in that In step 3, the time for dissolving the magnetic separation slag with water is 5 to 60 minutes.

Citation Information

Cited By

  • Method for recycling positive electrode material of lithium ion battery

    CN120413861A

  • Method for recycling lithium ion battery cathode material

    CN120413861B