Method for manufacturing ultra-fine pores in surface of LTCC (Low Temperature Co-Fired Ceramic) substrate
Through laser drilling and multi-layer sintering processes, the through hole diameter of the LTCC substrate is reduced to form ultra-fine holes, which solves the problem of excessive through hole diameter in the prior art, and achieves higher alignment tolerance and pad accuracy. Improve the assembly capability of high-density digital chips.
Patent Information
- Application Number
- CN202410928729.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-08
AI Technical Summary
The existing LTCC substrate process is difficult to produce fine pads with a diameter of less than 0.1mm, and the sintering shrinkage error results in poor size and position accuracy of the substrate surface pads, which cannot meet the needs of high-density digital chips, and the through-hole diameter is too large to meet the fine ones. The pad alignment tolerance requirements lead to uneven solder joints or short circuit problems.
Using laser drilling, porous stone vacuum table printing conductor paste, protective film lamination sintering and grinding polishing methods, the diameter of the through holes is reduced, ultra-fine micro-holes are formed, the micro-pad alignment tolerance range is widened, and the re-wiring capacity is improved. .
Reduce the through hole diameter below 0.03mm to significantly improve the alignment tolerance of the fine pads, improve the processing ability of the substrate arrayed fine pads, and avoid uneven solder joints or short circuit problems.
Smart Images

Figure CN118921848A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of LTCC circuit substrate manufacturing, and in particular to a method for manufacturing ultrafine pores on the surface of a LTCC substrate. Background Art
[0002] LTCC (low temperature co-fired ceramics) are widely used in microwave / millimeter wave communications. However, as the communications field continues to move towards high density, multi-function and digitalization, flip-chip integration of RF chips, digital chips, control chips, etc. on a single substrate has become a clear trend.
[0003] The traditional LTCC substrate process makes it difficult to produce fine pads with a diameter of less than 0.1mm, and the substrate has a sintering shrinkage error of ±0.2% to ±0.3%. These characteristics result in poor dimensional and positional accuracy of the co-fired pads on the substrate surface, which cannot meet the needs of high-density flip-chip assembly of large-size digital chips (size 20mm to 30mm, or even higher).
[0004] To address this issue, the industry has used the LTCC / D process (LTCC surface thin film process rewiring) on the surface of the LTCC substrate to produce micro pads that are interconnected with the co-fired through-holes of the substrate through rewiring, thereby improving the size and position accuracy of the surface pads.
[0005] However, for high-density digital flip-chip integration, the pad array area of a single chip will reach 30mm or even higher. Calculated based on the sintering shrinkage deviation of ±0.2%, the position deviation between the farthest through holes can reach more than 0.06mm, which means that the single-sided interconnection tolerance between the pad with a diameter of 0.1 and the through hole must reach more than 0.03mm to achieve full coverage of the through hole by the rewiring fine pad. Under normal circumstances, the through hole diameter of the LTCC substrate is ≥0.07mm. Compared with the pad with a diameter of 0.1mm, the single-sided interconnection tolerance is only 0.015mm, which cannot meet the process tolerance requirements. Some through holes will be exposed outside the pad, resulting in an increase in the equivalent pad and a decrease in the equivalent interconnection pitch. It is easy to cause problems such as uneven solder joints or welding short circuits during flip-flop welding.
[0006] Since the fluctuation of LTCC sintering shrinkage rate is an inherent characteristic of this type of commercial material and it is difficult to reduce it, when the size of the fine pad cannot be expanded, the more effective way to improve the alignment tolerance of the pad and the through-hole interconnection is to reduce the through-hole diameter. However, since it is an emerging demand, there is little research in this area in the industry. The patent "Control Method for Sintering Flattening of Multi-layer Through-hole Stacking on LTCC Substrates" discloses a method of improving the sintering flatness of through-holes by leveling and scraping holes, but it is still a conventional LTCC through-hole and does not mention the reduction of through-hole diameter; the patent "A transitional hole-filling slurry for connecting the upper and lower gold and silver layers of the film strip in the LTCC substrate" and the patent "A hole-filling gold paste and preparation method for LTCC substrates" both disclose the formula and preparation method of the hole-filling slurry, but they are all applied to conventional LTCC through-holes and do not involve the reduction of through-hole diameter. The patent "A method for producing an ultra-thin, high-density, multi-layer interconnected ceramic substrate" discloses a method of using a laser to drill holes in a ceramic sheet and then using sputtering and electroplating to metallize the holes to produce an ultra-thin, high-density multi-layer substrate, but does not mention the reduction in through-hole diameter, and the process method used is not applicable to LTCC substrate processing; the paper "The influence of glass powder on the performance of through-hole silver paste for low-temperature co-firing" studies the influence of glass powder softening point and addition amount on through-hole silver paste, but does not mention the production of small holes; the paper "Research on CO2 laser direct through-hole drilling process for packaging substrates" studies the application of CO2 laser direct through-hole drilling process in special copper-clad laminates, but the achieved through-hole diameter is 70μm, which cannot meet the demand for ultra-fine holes, and its production process is not applicable to LTCC substrate processing; the paper "Eliminating open-circuit failures between through-holes and conduction bands by controlling the shrinkage rate of multi-layer substrates" eliminates open-circuit failures by adjusting the densification temperature of wiring metal and ceramic materials and the shrinkage rate of substrates, but does not mention small hole processing.
[0007] In order to solve the problem that the through-hole size of conventional LTCC substrates is too large to meet the tolerance requirements of through-hole interconnection for arrayed micro-pads, it is urgent to develop a method for making ultra-fine holes on the surface of LTCC substrates, reduce the diameter of the surface through-holes, widen the alignment tolerance range with the re-wiring micro-pads, and improve the re-wiring capability of arrayed micro-pads. Summary of the invention
[0008] In order to solve the above problems, the present invention proposes a method for manufacturing ultra-fine micropores on the surface of an LTCC substrate, which can realize ultra-fine micropore processing on the substrate surface and widen the alignment tolerance capability of the surface through hole and the rewiring fine pad.
[0009] The technical solution adopted by the present invention is as follows:
[0010] A method for manufacturing ultra-fine pores on the surface of a LTCC substrate, comprising:
[0011] The raw porcelain is stripped and aged, and the raw porcelain is drilled with laser;
[0012] The punched green porcelain is adsorbed on a porous stone vacuum table, and a large area of conductive slurry is printed on the surface of the green porcelain, and then fixed and dried;
[0013] A slightly sticky protective film is pasted on the raw porcelain surface printed with a large area of conductive paste;
[0014] The multi-layer green porcelain with protective film is aligned and forcedly laminated, and the laminated green porcelain is sintered to transform the green porcelain into a dielectric, and the conductor slurry into a wiring film layer and through-hole with high conductivity to form an LTCC substrate;
[0015] The surface of the LTCC substrate is ground and polished to obtain an LTCC substrate with ultrafine pores on the surface.
[0016] Furthermore, the demolding and aging of the green porcelain includes: tearing off the PET film on the back of the green porcelain, baking the green porcelain at a set temperature, and then leaving it to stand at room temperature to fully release the casting stress of the green porcelain itself.
[0017] Furthermore, the method of drilling holes in the green porcelain using a laser includes: drilling holes in the green porcelain using an ultraviolet nanosecond or ultraviolet picosecond laser, so that the through-hole positions of the green porcelain are drilled through to form through-holes.
[0018] Furthermore, the punched green porcelain is adsorbed on a porous stone vacuum table, and a large area of conductor slurry is printed on the surface of the green porcelain, including: forming a funnel-shaped through-hole filling at the position of the green porcelain through-hole by screen printing and vacuum adsorption.
[0019] Furthermore, the fixing and drying includes: after large-area printing on the surface, the raw porcelain is always adsorbed and fixed on the porous stone vacuum table, and then the raw porcelain is heated with an infrared baking lamp to dry the printed slurry to prevent the raw porcelain with its own PET film from being deformed during the drying of large-area conductor slurry.
[0020] Furthermore, the alignment method of the alignment stack includes: equipment optical alignment and pin hole alignment.
[0021] Furthermore, the forced lamination includes: placing a stainless steel sheet above the surface green porcelain protective film to achieve extrusion of the surface conductor slurry into the through hole during the lamination process.
[0022] Furthermore, the sintering of the laminated green porcelain includes: sintering the laminated green porcelain using a conventional LTCC sintering process compatible with the material, so that the green porcelain is converted into a dielectric, and the conductor slurry is converted into a wiring film layer and through holes with high conductivity to form an LTCC substrate.
[0023] Furthermore, the grinding includes: grinding and thinning the upper surface of the LTCC substrate, removing the large-area metal layer printed on the surface, exposing the metallized micropores in the surface layer medium to the surface, and forming ultra-fine micropores on the surface of the LTCC substrate.
[0024] Furthermore, the polishing includes: performing a polishing process on the ground LTCC substrate surface to reduce the substrate surface roughness and provide a good surface state for rewiring.
[0025] The beneficial effects of the present invention are:
[0026] The present invention proposes a method for making ultra-fine holes on the surface of LTCC substrates, which can realize ultra-fine hole processing on the surface of the substrate and widen the alignment tolerance capability of the surface through-holes and the rewiring fine pads. The present invention can reduce the diameter of the through-holes on the surface of the substrate from the conventional 0.07mm or more to less than 0.03mm, which can greatly improve the alignment tolerance of the surface through-holes and the rewiring of the surface fine pads, and improve the processing capability of the substrate array fine pads. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of raw porcelain demolding aging and laser micro-hole processing.
[0028] Figure 2 Schematic diagram of large-area printing for adsorption.
[0029] Figure 3 Schematic diagram of fixed drying after large-area printing.
[0030] Figure 4 This is a schematic diagram of film protection.
[0031] Figure 5 Schematic diagram of the film stack.
[0032] Figure 6 Schematic diagram of forced lamination.
[0033] Figure 7 Schematic diagram of the cross section of the raw porcelain block after lamination.
[0034] Figure 8 Schematic diagram of the cross section of the LTCC substrate after sintering of the green ceramic block.
[0035] Fig. 9 This is a schematic cross-sectional view of the LTCC substrate surface after grinding and polishing.
[0036] Fig.10 Schematic diagram of the cross-section of the rewiring of fine pads on the surface of the LTCC substrate.
[0037] Figure numerals: 1 is raw porcelain, 1-1 is the first layer of medium after sintering, 2 is the PET film on the back of the raw porcelain, 3 is the porous stone vacuum table for adsorbing and fixing the raw porcelain during printing, 3-1 is the downward adsorption force generated by the porous stone, 4 is the PET micro-adhesive film attached to the large-area conductor film layer m1 on the raw porcelain 1, 5 is the forced laminated stainless steel sheet, 5-1 is the lamination pressure, 6 is the laminated stainless steel back plate; G is the raw porcelain with its own PET film, V0 is the fine through hole processed on the raw porcelain by laser; P is the printing paste, S1 is the printing screen, S2 is the printing Brush scraper, m1 is the large-area conductor slurry layer printed on the surface of green porcelain 1, V1 is the fine through hole after partial filling of slurry; ML is other wiring layers of LTCC substrate, L is the conventional wiring inside the substrate, K is the conventional through hole inside the substrate; V2 is the fine through hole after further filling of slurry; m1-1 is the large-area conductor film layer on the surface of LTCC substrate after sintering, V3 is the ultra-fine pore on the surface dielectric layer after sintering, L-1 is the conventional wiring inside the LTCC substrate after sintering, and K-1 is the conventional metallized through hole inside the LTCC substrate after sintering. DETAILED DESCRIPTION
[0038] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] like Figure 1 As shown, this embodiment provides a method for making ultra-fine pores on the surface of a LTCC substrate, including raw porcelain stripping aging and laser micropore processing, adsorption large-area printing and fixed drying, raw porcelain surface film protection, film lamination, forced lamination and co-firing, LTCC substrate surface grinding and polishing, etc. The specific implementation process is as follows:
[0041] Raw porcelain demolding and aging and laser micro-hole processing: demolding and aging of raw porcelain, and drilling of raw porcelain by laser;
[0042] Adsorption of large-area printing and fixed drying: The punched raw porcelain is adsorbed on the porous stone vacuum table, and a large area of conductor slurry is printed on the surface of the raw porcelain, and then fixed and dried;
[0043] Film protection on raw porcelain surface: A slightly sticky protective film is pasted on the raw porcelain surface printed with a large area of conductive paste;
[0044] Film stacking, forced lamination and co-firing: The multi-layer green porcelain with protective film is aligned and forcedly laminated, and the laminated green porcelain is sintered to transform the green porcelain into a dielectric, and the conductor slurry into a routing film layer and through-hole with high conductivity to form an LTCC substrate;
[0045] LTCC substrate surface grinding and polishing: The surface of the LTCC substrate is ground and polished to obtain an LTCC substrate with ultra-fine pores on the surface.
[0046] Preferably, the green porcelain demolding and aging refers to selecting green porcelain with a thickness not exceeding 0.05 mm, tearing off the PET film on the back thereof, and baking the green porcelain at a temperature of 80°C to 90°C for 10 min to 30 min, and then leaving it to stand at room temperature for 24 h to 48 h, so that the casting stress of the green porcelain itself can be fully released and the deformation in subsequent processing can be reduced.
[0047] Preferably, laser micro-hole processing refers to using ultraviolet nanosecond or ultraviolet picosecond laser to punch holes in green porcelain, with a processing power of 3W to 5W and 5 to 20 processing times to ensure that the through-hole positions of the green porcelain are punched through to form through-holes.
[0048] Preferably, adsorption large-area printing means horizontally adsorbing the green porcelain on a porous stone vacuum table, and then printing a large area of conductive slurry on the surface of the green porcelain, with a wet film thickness of 10 μm to 30 μm, and forming a funnel-shaped through-hole filling at the through-hole position through vacuum adsorption.
[0049] Preferably, fixed drying is different from the conventional LTCC printing drying process in which free-state raw porcelain is baked in an oven. Here, it means that after large-area printing on the surface, the raw porcelain is always adsorbed and fixed on the porous stone vacuum table, and then the raw porcelain is heated with an infrared baking lamp to dry the printed slurry to prevent the raw porcelain with its own PET film from being deformed during the drying of large-area conductor slurry.
[0050] Preferably, the surface protection of raw porcelain refers to sticking a layer of slightly sticky PET film on the surface of the large-area conductor layer printed on the raw porcelain. The thickness of the PET film is 0.05mm to 0.1mm. The slight stickiness of the surface can not only restrain the deformation of the raw porcelain, but also enable it to be smoothly peeled off from the raw porcelain after lamination.
[0051] Preferably, the conventional LTCC process of lamination with film and demolding before lamination is different. Here, the surface layer of green ceramic is aligned with other layers of green ceramic with a protective film. The alignment method can be optical alignment of the equipment or pin hole alignment.
[0052] Preferably, forced lamination means placing a stainless steel sheet with a thickness of 0.1 mm to 0.3 mm above the surface green porcelain protective film during the lamination process, so as to achieve an extrusion effect on the surface conductor paste into the through hole during the lamination process.
[0053] Preferably, co-firing refers to sintering the laminated LTCC green ceramic blocks using a conventional LTCC sintering process that is compatible with the material, so that the green ceramic is converted into a dielectric, and the conductor paste is converted into a routing film layer and through holes with high conductivity, thereby forming an LTCC circuit substrate.
[0054] Preferably, grinding refers to grinding and thinning the upper surface of the LTCC substrate to remove the large-area metal layer printed on the surface, so that the metallized micropores in the surface layer medium are exposed to the surface, forming ultrafine micropores on the substrate surface.
[0055] Preferably, polishing refers to polishing the surface of the ground LTCC substrate to reduce the surface roughness of the substrate and provide a good surface state for rewiring. If the surface roughness of the ground substrate meets the rewiring requirement, the polishing process can be omitted.
[0056] Preferably, after the surface ultrafine pore processing is completed, a micro pad array with high dimensional accuracy and high positional accuracy can be arranged on the surface of the LTCC substrate through a thin film process or a 3D printing process.
[0057] Example 2
[0058] This embodiment is based on embodiment 1:
[0059] This embodiment provides a method for manufacturing ultra-fine pores on the surface of a LTCC substrate, comprising the following steps:
[0060] like Figure 1 As shown in the figure, a 951 type green porcelain 1 with a thickness of 0.05 mm was selected, the PET film on the back was torn off, and the green porcelain was baked at 85°C for 20 minutes in a hot air oven and left to stand at room temperature for 30 hours. Then, a UV picosecond laser was used to punch holes in the green porcelain, with a processing power of 4W and 15 processing times, completing the processing of a through hole V0 with a diameter of 0.03 mm.
[0061] like Figure 2 As shown, the raw porcelain 1 is vacuum-adsorbed on the porous stone table 3, and a large-area printing is performed on the surface of the raw porcelain 1 using a printing screen S1, a printing scraper S2 and a printing paste P to form a large-area conductive paste layer m1 and fine through holes V1 partially filled with the paste. The wet film thickness of the large-area conductive paste layer m1 is 23μm to 26μm.
[0062] like Figure 3As shown, under vacuum adsorption and fixation, the large-area conductive paste layer m1 and the fine through-holes V1 on the green porcelain 1 are dried.
[0063] like Figure 4 As shown, under vacuum adsorption and fixation, a PET micro-adhesive film 4 is pasted on the large-area conductive paste layer m1 to protect the raw porcelain, and the thickness of the PET micro-adhesive film 4 is 0.05 mm.
[0064] like Figure 5 As shown, the raw porcelain 1 is set as the surface raw porcelain of the LTCC substrate, and is aligned and stacked with other wiring layers ML of the substrate under the protection of the PET micro-adhesive film 4. The material of other wiring layers ML is still 951 type raw porcelain, and the thickness of a single layer of raw porcelain is the conventional 0.127mm. The conventional wiring L in the inner layer of the substrate and the conventional through hole K inside the substrate are all made using the conventional LTCC process.
[0065] like Figure 6 As shown, the laminated raw porcelain is placed on a laminated stainless steel back plate 6, and a 0.2 mm thick forced laminated stainless steel sheet 5 is placed on the upper surface. After the whole is vacuum packed, it is laminated using warm water isostatic pressing. The lamination temperature is 70°C, the lamination pressure is 3000PSI, and the lamination time is 15 minutes. 5-1 is a schematic diagram of the application of lamination pressure.
[0066] like Figure 7 As shown in FIG. 1 , after forced lamination, the surface partially filled micro-vias are transformed into fully filled micro-vias V2 through the migration of the slurry in the large area conductive slurry layer m1. The laminated green ceramic block is sintered to form an LTCC substrate such as Figure 8 As shown, 1-1 is the first dielectric layer after sintering, m1-1 is the large-area conductor film layer on the surface of the LTCC substrate after sintering, V3 is the ultra-fine pores on the surface dielectric layer after sintering, L-1 is the conventional wiring inside the LTCC substrate after sintering, and K-1 is the conventional metallized through hole inside the LTCC substrate after sintering.
[0067] like Fig. 9 As shown, the LTCC substrate is ground and polished to remove the large-area conductor film layer m1-1 on the surface, so that the ultra-fine pores V3 in the first layer of dielectric 1-1 are exposed on the substrate surface, forming surface metallized ultra-fine pores with a pore diameter of 0.025mm-0.028mm.
[0068] like Fig.10 As shown in the figure, on the ultra-fine pores on the surface of LTCC, a fine pad with a diameter of 0.1mm is made using a thin film wiring process, and good coverage of the micropores by the rewiring pad is achieved in the range of 35mm×35mm.
[0069] It should be noted that, for the aforementioned method embodiments, for the sake of simplicity of description, they are expressed as a series of action combinations, but those skilled in the art should be aware that the present application is not limited by the order of the actions described, because according to the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present application.
Claims
1. A method for making ultrafine pores on the surface of a LTCC substrate, characterized in that: include: The raw porcelain is stripped and aged, and the raw porcelain is drilled with laser; The punched green porcelain is adsorbed on a porous stone vacuum table, and a large area of conductive slurry is printed on the surface of the green porcelain, and then fixed and dried; A slightly sticky protective film is pasted on the raw porcelain surface printed with a large area of conductive paste; The multi-layer green porcelain with protective film is aligned and forcedly laminated, and the laminated green porcelain is sintered to transform the green porcelain into a dielectric, and the conductor slurry into a wiring film layer and through-hole with high conductivity to form an LTCC substrate; The surface of the LTCC substrate is ground and polished to obtain an LTCC substrate with ultrafine pores on the surface.
2. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The stripping and aging of the green porcelain comprises: tearing off the PET film on the back of the green porcelain, baking the green porcelain at a set temperature, and then leaving it to stand at room temperature to fully release the casting stress of the green porcelain itself.
3. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The method of drilling holes in green porcelain using laser includes: drilling holes in green porcelain using ultraviolet nanosecond or ultraviolet picosecond laser, so that the through-hole positions of green porcelain are drilled through to form through-holes.
4. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The punched green porcelain is adsorbed on a porous stone vacuum table, and a large area of conductor slurry is printed on the surface of the green porcelain, including: forming a funnel-shaped through-hole filling at the position of the green porcelain through-hole by screen printing and vacuum adsorption.
5. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The fixing and drying comprises: after large-area printing on the surface, the raw porcelain is always adsorbed and fixed on the porous stone vacuum table, and then the raw porcelain is heated with an infrared baking lamp to dry the printed slurry, so as to prevent the raw porcelain with its own PET film from being deformed during the drying of large-area conductor slurry.
6. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The alignment method of the alignment stack includes: equipment optical alignment and pin hole alignment.
7. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The forced lamination includes: placing a stainless steel sheet above the surface raw porcelain protective film to achieve extrusion of the surface conductor slurry into the through hole during the lamination process.
8. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The sintering of the laminated green porcelain includes: sintering the laminated green porcelain using a conventional LTCC sintering process compatible with the material, so that the green porcelain is converted into a dielectric, and the conductor slurry is converted into a wiring film layer and a through hole with a high conductivity function, so as to form an LTCC substrate.
9. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The grinding includes: grinding and thinning the upper surface of the LTCC substrate, removing the large-area metal layer printed on the surface, exposing the metallized micropores in the surface layer medium to the surface, and forming ultra-fine micropores on the surface of the LTCC substrate.
10. The method for making ultrafine pores on the surface of a LTCC substrate according to claim 1, characterized in that: The polishing includes: polishing the ground LTCC substrate surface to reduce the substrate surface roughness and provide a good surface state for rewiring.