Method for manufacturing shaving board and shaving board
By using high proportional adhesives and thermoset/thermoplastic components in particleboard manufacturing, the problem of insufficient strength and water resistance of particleboard is solved, and the effect of high strength and reversible expansion is achieved, expanding its application range.
Patent Information
- Application Number
- CN202380026761.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-10
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-08
AI Technical Summary
Existing particleboards are limited in industrial and construction industries, and long-term use is almost impossible in external areas due to their limited strength and poor water resistance.
The thermal pressing is performed to improve the strength and water resistance of the particleboard by using a high proportion of adhesive calculated relative to the absolute dry wood, combining the thermoset and thermoplastic components of the adhesive in the process of manufacturing the particleboard.
The high strength and good water resistance of particleboard are achieved, and the expansion property becomes reversible. The particleboard can completely restore its initial size after water soaking, expanding its application field.
Smart Images

Figure CN118922284A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing a particle board and a particle board. Background Art
[0002] A method of the type mentioned at the outset is used for pressing chipboards from wood, for example from round wood, new wood, old wood or residual wood or from annual plants, for example straw or bagasse, and from sawdust and / or sawdust.
[0003] To produce particleboard, wood, for example round or old wood or annual plants, is comminuted into chips in a first comminution step, for example in a knife-ring flaker. To produce fine chips, the chips can be further comminuted, for example in a dual-flow grinder or an impact grinder. The chips are usually dried before being temporarily stored in a silo. Single-lane or triple-lane drum dryers or belt dryers are usually used for this purpose.
[0004] Before pressing in the press, the chips are graded, for example, by means of a mechanical sieve or by means of a blower, and glued with an adhesive. When gluing the chips, a proportion of 2 to 11% by weight of adhesive, calculated relative to the absolutely dry wood, is usually used. The glued chips are spread, for example, by means of wind, throwing or rolling methods, and the chip block thus formed is subsequently pressed into particleboard, for example in a continuous and / or discontinuous press.
[0005] Particle boards produced by known methods are used in various forms in many industries and construction sectors, in particular for interior decoration or the furniture industry. However, particle boards have only limited strength and poor water or moisture resistance, which significantly limits their range of applications. Long-term or even permanent use in exterior areas is virtually impossible with known, possibly jacketed particle boards. Summary of the invention
[0006] The object of the present invention is to provide a method in which a particle board with improved properties, in particular with increased strength, can be produced. The object of the present invention is also to provide improved properties of a particle board, in particular with increased strength.
[0007] This object is achieved by a method for producing a particle board according to claim 1 and a particle board according to claim 13. The dependent claims relate to advantageous developments of the invention.
[0008] The method for producing a particle board according to the invention comprises the following steps:
[0009] - provide chips obtained from wood;
[0010] - providing at least one adhesive,
[0011] - applying a binder to the chips, wherein a proportion of the binder, calculated on the absolutely dry wood, of at least 12% by weight is applied to the chips;
[0012] - forming one or more layers of chip blocks,
[0013] - Pressing of chip blocks in a hot press to produce particleboard.
[0014] The steps of the method correspond to the steps of conventional methods for producing planar extruded boards, for example. However, according to the invention, an adhesive portion of at least 12% by weight is used, calculated relative to absolutely dry wood. Based on the portion of the chips, preferably an adhesive portion of at least 15% by weight, calculated relative to absolutely dry wood, preferably an adhesive portion of at least 17% by weight, calculated relative to absolutely dry wood, particularly preferably an adhesive portion of at least 20% by weight, calculated relative to absolutely dry wood, and very particularly preferably a minimum of 25% by weight, calculated relative to absolutely dry wood, is applied to the chips. Under the premise of ensuring that the moisture content of one layer and / or multiple layers of the chip block after gluing does not exceed the upper limit, any high adhesive portion can be applied to the chips. Preferably, the upper limit of the moisture content is between 1% by weight, calculated relative to the glued wood, and 20% by weight, calculated relative to the glued wood, preferably between 3% by weight, calculated relative to the glued wood, and 18% by weight, calculated relative to the glued wood, and particularly preferably between 5% by weight, calculated relative to the glued wood, and 15% by weight, calculated relative to the glued wood.
[0015] The binder content is expressed on a chip basis, i.e. the binder content is expressed on the basis of the weight of the chip used. For chips that can absorb moisture (e.g. wood chips), the binder content is calculated based on wood that has been dried to constant weight. The chips are dried to constant weight at 103±2°C and are referred to as atro wood (atro wood: absolutely dry wood). The binder content is taken as 100% solids, i.e. without any liquid that may have been added.
[0016] In order to provide cuttings, wood cellulose materials, such as wood, such as round wood, new wood, old wood or residual wood or annual plants, typically straw or bagasse, are pulverized in a single-step or multi-step cutting operation. Typical devices for cutting wood are, for example, drum slicers and disc slicers and knife ring flakers. In addition to the cuttings obtained from cutting, sawdust and sawdust can also be provided, for example. Preferably, these cuttings have a length of 0.5mm to 50mm, a width of 0.1mm to 20mm, and a thickness of 0.05mm to 2mm. Here, it is usually distinguished into coarse cuttings with a length of 5mm to 50mm, a width of 1 to 20mm, and a thickness of 0.2 to 2mm, and fine cuttings with a length of 0.5mm to 25mm, a width of 0.1 to 5mm, and a thickness of 0.05 to 1mm.
[0017] If the chips contain moisture, such as is typical for wood chips made from new wood, the moisture content should be adjusted before pressing the chip block so that after pressing, in particular if the climatic conditions remain unchanged without water storage, a dimensionally stable particleboard that does not expand or shrink is obtained. During the pressing process, for example in the particleboard process, the chips preferably have a moisture content of 1% by weight, calculated on absolutely dry wood, to 4% by weight, calculated on absolutely dry wood, before gluing. To adjust the desired moisture content, the chips are dried.
[0018] Before or preferably after drying, the chips can be sorted, for example sieved. During the sorting, the chips are divided, for example, into four fractions (dust, fine chips, coarse chips and oversized chips). Dust is preferably separated from the other fractions and is preferably utilized in terms of energy. Oversized and / or coarse chips can be sieved out and preferably re-comminuted.
[0019] The inventors have recognized that the use of a high proportion of adhesive in the particleboard gluing process can produce a particleboard with water resistance and corresponding moisture resistance, while this particleboard also has a very high strength. In addition, it was surprisingly found that the expansion of the particleboard, for example after 24 hours of water immersion, becomes reversible due to the high adhesive ratio through a high proportion of adhesive content. The determination of the expansion behavior is preferably carried out according to the DIN EN 317 standard. After 24 hours of return drying, for example at room temperature, the particleboard has reached its initial dimensions again, for example the initial length, initial width and initial thickness before 24 hours of water storage. It can be inferred from this that the adhesive compound remains essentially undamaged during the action of water. So far, this expansion disappearance characteristic has not been observed in particleboards, but what usually occurs is a partially irreversible residual deformation. By completely restoring the deformation produced by expansion, new application areas can be opened up for particleboards.
[0020] Particularly preferably, for the production of particleboards, an adhesive is used which has a first thermosetting component and a second thermoplastic component. The proportion of adhesive is at least 12% by weight, calculated on the basis of the absolutely dry wood, to 60% by weight, calculated on the basis of the absolutely dry wood, preferably 15% by weight, calculated on the basis of the absolutely dry wood, to 45% by weight, calculated on the basis of the absolutely dry wood, particularly preferably 18% by weight, calculated on the basis of the absolutely dry wood, to 35% by weight, calculated on the basis of the absolutely dry wood, in particular 20% by weight, calculated on the basis of the absolutely dry wood, to 33% by weight, advantageously 24% by weight, calculated on the basis of the absolutely dry wood, to 31% by weight.
[0021] According to an advantageous embodiment of the invention, condensation resins, in particular aminoplasts, such as melamine-formaldehyde resins, urea-formaldehyde resins (UF resins) or benzoguanamine resins, and phenolic resins, such as phenol-formaldehyde resins (PF resins), are used as the first thermosetting component of the adhesive, either alone or in a mixture. The aminoplasts are used in aqueous solution, for example as melamine resins, usually as melamine-formaldehyde resins (MF resins), wherein the solids content of the aminoplasts is preferably at least 45% by weight, calculated on the basis of the aqueous solution; advantageously, the solids content is more than 50% by weight. The upper limit of the solids content is determined by the solubility and, if necessary, the processability of the aminoplasts during the production process, for example in nozzle or high-pressure gluing methods.
[0022] Preferably, the adhesive has a melamine resin as at least a first component, for example as a MF resin (melamine formaldehyde resin). Melamine resin is preferred because it has low expansion and low hygroscopicity and is resistant to hydrolysis. Alternatives are phenolic resins, urea-formaldehyde resins or a mixture or combination of a variety of these thermosetting first components. Although urea-formaldehyde resins are not resistant to hot water, it can surprisingly be used in particular with a mixture of melamine resins and / or phenolic resins for the manufacture of particleboards according to the invention. In particular, melamine resins can be used alone as a first component or in combination with one or more other thermosetting components. The proportion of UF resin is preferably at most 50% by weight of the MF or PF resin without impairing the water resistance or water resistance of the particleboard.
[0023] In the context of the present invention, combination means that a mixture of resins of the first component can be used, wherein a mixture of two or more resins of the first component is applied to the chips simultaneously. Or a plurality of different resins of the first component are used in sequence, for example because they cannot be used in the form of a mixture or because separate application of different resins of the first component or individual resins of the first component of the adhesive has a favorable effect, for example on the subsequent product properties and / or application properties.
[0024] Preferably, technical grade diphenylmethane diisocyanate (PMDI) is applied to the above-mentioned chips as the second thermoplastic component of the adhesive. As its replacement or supplement, other substances can also be used, such as distyrene isocyanate (MDI), which can also be used as eMDI in an emulsified form, and polyurethane can also be used as the second component. The share of the second component is preferably greater than 1% by weight, especially 3% by weight or more, advantageously 5% by weight or more, calculated based on absolutely dry wood. Therefore, in the particleboard according to the present invention, the share of the second component such as PMDI is significantly higher than conventional particleboard. Advantageously, the second component of the adhesive, such as PMDI, is also used in the case of the multilayer structure of the board, or is especially used in the covering layer of the particleboard according to the present invention. The second component is preferably used in the middle layer and the covering layer with the same amount. Here, a variety of substances that are equally suitable as the second component can be applied to the chips in a mixed manner or individually in sequence.
[0025] Preferably, at least one third component, such as a polyol or a polyether, can be added to the first component and the second component of the adhesive, preferably as a solid, respectively. The third component can be added in a proportion of up to 15% by weight, preferably up to 10% by weight, particularly preferably 2 to 5% by weight, based on the total amount of the adhesive.
[0026] According to an advantageous embodiment, the elastic properties of the particleboard can be modified, in particular improved, by adding an elastomer or thermoplastic, which serves as an elasticizing additive, for example by adding polyvinyl acetate (PVAc) or ethylvinyl acetate. It is particularly preferred that the elastomer or thermoplastic is applied to the chips as an elasticizing additive, in particular in addition to the first and second components of the adhesive. Advantageously, the elasticizing additive is not added to the first or second component of the adhesive or is not applied to the chips together with one of the components of the adhesive. Acrylates, styrene acrylates or polyurethanes (PU) are preferably used for elasticizing the particleboard according to the invention, in particular in the form of liquid additives such as dispersions or emulsions, because they are water-resistant. Acrylates, styrene acrylates and PU are preferably used with a glass transition temperature Tg of less than 0° C. However, mono- or diethylene glycol is also suitable for elasticizing the particleboard. The above-mentioned elasticizing additives can be used individually or in mixed form. The addition of elastomers or thermoplastics reduces the brittleness of the particleboard and improves its elastic properties, such as the modulus of elasticity. In addition, the addition of an elasticizing additive improves the flatness of the particleboard according to the invention. The elasticizing additive is preferably used in an amount of 1% to 7% by weight, advantageously 2% to 7% by weight, preferably 2% to 6% by weight, particularly preferably 2.5% to 5.5% by weight, based on the total amount of the particleboard (absolutely dry), calculated as a solid. The elasticizing additive is added, for example, to an adhesive, such as a melamine resin, before applying to the chips and is applied to the chips together with the adhesive. Preferably, the elasticizing additive is applied to the chips before or more preferably after applying the adhesive.
[0027] As described above, the first component and the second component, and optionally more components, are combined as an adhesive. Preferably, the adhesive mainly comprises the first component, especially a melamine resin. Further preferably, the first component accounts for more than 15% by weight, especially 20% by weight of the total use of the adhesive. The first component and the second component of the adhesive can be adjusted steplessly in a wide range according to the requirements of the particleboard. This preferably means that in a multilayer board structure, it is applicable to both the middle layer and the other layers. They are preferably applied to the chips in a ratio of 2:1, preferably 3:1, particularly preferably 4:1 or 5:1 of the first component to the second component or in a ratio between these values. If the particleboard according to the present invention has a covering layer, it is preferred to use a higher proportion of the first component of the adhesive compared to the middle layer.
[0028] Adhesive is usually provided in liquid form, but can also exist in solid form, for example in the form of particles or powder. Adhesive can be provided in pure form, or usually in liquid form in solvent or in water as dispersion or emulsion according to the proportion. In the context of the present invention, adhesive is always based on 100% solid, i.e. without solvent or water proportion for example. The application of adhesive on the cuttings, especially the application is mostly realized by spraying, for example by a plurality of nozzles, for example high-pressure nozzles, which produce the spray of adhesive and can for example be arranged around the downstream of the cuttings. The typical embodiment of this gluing device is for example a so-called downfeed channel, and / or additionally a traditional gluing mixer used in particleboard manufacturing. Coarse cuttings are preferably glued in the downfeed channel, and then guided through a traditional gluing mixer, wherein, in the gluing mixer, preferably one or more adhesive components are applied. Fine cuttings are glued in a traditional gluing mixer and / or downfeed channel.
[0029] The surface of the chips is wetted with adhesive drops or with an adhesive mist. The chips wetted with adhesive are formed into chip blocks and then pressed. In this case, when a thermosetting adhesive is used, the adhesive hardens under the action of increased pressure and increased temperature; it polymerizes, for example, in an irreversible addition or condensation reaction. If a thermoplastic adhesive is used, it solidifies thermally reversibly. The thermoplastic adhesive is mechanically anchored to the chips during pressing. The two components of the adhesive are preferably used in combination with one another.
[0030] The adhesive can be applied to the chips preferably in one process or in multiple processes, depending on the type, amount or combination of the components of the adhesive. Possibly, the chips can be dried after applying, for example, one component of the adhesive.
[0031] As is common in chips, the formation of chip blocks is usually carried out by spreading, for example by means of wind spreading methods and / or throwing spreading methods. The chips glued with the entire amount of adhesive are spread on a carrier, usually on a conveyor belt, for example in a uniform layer, or in multiple layers, wherein the layers can have different compositions related to chips, adhesives, elasticizing additives or additives as necessary. The scattered chip blocks are first pre-compacted on the carrier by a pre-pressing machine if necessary, and then pressed in a press. Here, the press acts on the upper and lower sides of the chip block or particle board by means of a pressing element, such as a pressing plate or a pressing belt. During the hardening or solidification that is basically carried out on the upper and lower sides of the chip block under the action of pressure and temperature, a particle board with a width given by the press and a length if necessary is produced, or a particle board with an infinite length and a thickness given by the spacing of the pressing elements in a continuous press.
[0032] In principle, any press which applies pressure and temperature in a sufficient manner is suitable for producing particleboards, both board presses, in which the chip block or particleboard is pressed between two board materials, and continuous hot presses, for example continuous double-belt hot presses in the form of a circulating, heated metal press belt. In this press, the chip block or particleboard is pressed between two circulating press belts and the formed particleboard is conveyed through the press by the circulating press belt at a predetermined speed. Preferably, a hot press is used, the pressing elements of which, for example, in the form of a pressing plate or a circulating press belt, are heated to a predetermined temperature. Suitable pressing temperatures, measured as the temperature of the pressing element, can be from 150° C. to 240° C., preferably from 160° C. to 220° C. The thinner the board, the lower the pressing temperature that can be selected. Suitable pressing pressures are, for example, in the range of 2 N / mm 2 Up to 5N / mm 2 , preferably 3N / mm 2 Up to 5N / mm 2 , particularly preferably 3.5 N / mm 2 Up to 5N / mm 2 within the range.
[0033] The pressing factor, i.e. the time during which the pressing element acts on the chip block, is advantageously at least 6 seconds / mm of board thickness (hereinafter referred to as s / mm) up to 20 s / mm, preferably 8 s / mm to 18 s / mm, particularly preferably 9 s / mm to 15 s / mm. The pressing factor is thus significantly higher than that of comparable known standard particleboards of type P2 according to DIN EN 312, where the pressing factor is at most 5.5 s / mm.
[0034] It is particularly preferred that these chips or chip blocks are pressed into a particleboard with an odd number of layers. For example, the particleboard has three or five layers superimposed one above the other. In a particleboard with three layers, for example, the middle layer is arranged between two covering layers. Preferably, when forming the chip block, the chips are spread to form different layers. The covering layer preferably has fine chips for the most part, which are preferably spread by means of a wind spreading method. In the middle layer, a majority of coarse chips are preferably arranged, which are spread, for example, by means of a throwing method. The middle layer typically consists of a portion of the pressed particleboard of at least 30% by weight, preferably at least 45% by weight, and particularly preferably at least 60% by weight. The covering layers are symmetrically or asymmetrically spread with respect to their weight amount. If the particleboard according to the invention consists of a single-layer structure, the different chip portions of the above-mentioned coarse chips and fine chips are gathered in one layer.
[0035] A pre-press for compacting the chip mass can be provided before the actual hot pressing process. In principle, the separating agent can be applied, in particular sprayed, to the carrier, for example a conveyor belt or forming belt and / or the upper side of the mass. It is particularly preferred to apply the separating agent, for example a liquid with different polymers, in particular silicone, to the pressing elements of the press, thereby preventing the chip mass / chipboard from adhering to the pressing elements. For application to the pressing elements, the separating agent is preferably mixed with a fluid medium, in particular water.
[0036] Optionally, a device for cooling the particleboard can be connected downstream of the press, in particular a device for cooling at a predetermined pressing pressure can be connected downstream of the press, the predetermined pressing pressure can be less than the pressing pressure during pressing of the particleboard. Alternatively and / or additionally, the particleboard can be cooled at room temperature.
[0037] For the production of the particleboard according to the invention, one or more additives may also be used, such as antioxidants, light stabilizers, antistatic agents, colorants, bactericides, flame retardants, agents for adjusting the thermal or electrical conductivity, or one or more fillers. Mineral particles may be used as fillers, for example, but also ceramics, synthetic materials or particles made of glass or plastic. It is also possible to apply additives or combinations of fillers to the chips individually or as a mixture. Fillers and / or additives may also be applied, in particular applied, mixed with a binder.
[0038] According to an advantageous embodiment of the invention, a hydrophobizing agent is applied to the chips before the chips are pressed into the block, in particular after the chips have been glued. As hydrophobizing agents, for example paraffin or wax are provided, which are typically used in an amount of up to 5% by weight, calculated on the absolutely dry wood, usually in an amount of up to 2% by weight, calculated on the absolutely dry wood, usually in an amount of up to 0.1% by weight to 1% by weight, calculated on the absolutely dry wood, and if necessary in an amount of up to 1.5% by weight, calculated on the absolutely dry wood. The use of hydrophobizing agents helps to reduce the swelling tendency of the particleboard and to increase the moisture resistance of the particleboard.
[0039] According to an advantageous development of the invention, the particleboard is ground after pressing. For this purpose, a grinding device with grinding means, for example sandpaper and / or preferably a grinding belt, can be provided. Usually, the grinding is carried out in two grinding processes, wherein in the first grinding process grinding means with a grit of 50-60 are used and in the second grinding process grinding means with a grit of 80-100 are used. The particleboard according to the invention has a harder surface than the known particleboards according to DIN EN 312, wherein a coarser grit of the grinding means is preferred. Preferably, the grit in both grinding processes is a maximum of 60, preferably a maximum of 50, particularly preferably a maximum of 40.
[0040] The particleboard produced by the above method can be adapted to different requirements by different combinations of chips, adhesives, fillers and possibly other additives such as wax. It is therefore explicitly pointed out that the features described in conjunction with the present invention can be freely combined with each other.
[0041] The invention further relates to a particleboard having a binder content of at least 12% calculated relative to absolutely dry wood. The particleboard is produced in particular by the above-described method. The particleboard according to the invention is preferably waterproof and thus also moisture-proof. It has excellent and unusual expansion and contraction properties, which are manifested in a smaller expansion and a more complete expansion recovery during the subsequent drying process.
[0042] The particleboard according to the invention is constructed in the form of a board due to pressing, that is to say the particleboard has two main faces, which are also referred to as the upper side and the lower side in the following text. The upper side and the lower side are spaced apart from each other by the thickness of the particleboard. The narrow faces of the particleboard extend between the upper side and the lower side, which transition to the upper side and the lower side at the edges respectively. The thickness of the finished particleboard can be 2 mm to 80 mm, typically between 3 mm and 50 mm, mostly between 3 mm and 32 mm. Typical applications may require a particleboard thickness of 6 mm to 32 mm. The particleboard can have flat main faces; however, the upper side and / or the lower side can also be punched or milled or machined in another way, so that a variable thickness of the particleboard is produced relative to the surface of the particleboard.
[0043] Preferably, the particleboard has an odd number of layers in thickness. It is, for example, single-layer, three-layer or five-layer. The narrow sides of the particleboard according to the invention can be processed using common tools. They can be sawed, cut or milled. As required, for example, in the final manufacturing process, the particleboard can be cut off at its maximum length and width. Smaller sizes can be produced, for example, by disassembling the particleboard originally produced in a press. After being divided into floor panels, wall panels or ceiling panels, after production in a press, the typical size of the particleboard can be 6700mm (length) x 2500mm (width), and the size for floor, wall or ceiling panels after division is 1380mm x 195mm or 3048x 2800mm. Since the width of the board corresponds to the usual floor height, the latter specifications are particularly suitable for use in construction.
[0044] Advantageously, the particleboard according to the invention has only a very low thickness expansion, in particular according to the test method described in DIN EN 317, which is less than 5%, advantageously less than 4%, preferably less than 3%, particularly preferably less than 2.5% relative to the initial board thickness. It is also advantageous that an uncoated particleboard has an edge expansion according to the test method described in EN-13329 of less than 6%, preferably less than 5%, and a coated particleboard particularly preferably has an edge expansion of less than 4%. Compared to a standard particleboard of the same thickness made from the same chip material but with less use of adhesive and other types of adhesive, this expansion can be reduced by more than 90%. Values of less than 5% for edge expansion of uncoated particleboards and less than 4% for coated particleboards are therefore a particular improvement over the known particleboards according to DIN EN 312.
[0045] The average density of the particleboard according to the invention is preferably 800 kg / m 3 Up to 1000kg / m 3 , preferably 830kg / m 3 Up to 970kg / m 3 , particularly preferably 850kg / m 3 Up to 950kg / m 3 The average density is therefore about 100 kg / m higher than in the case of known particleboards of the P2 type according to DIN EN 312. 3 Up to 300kg / m 3 .
[0046] The particleboard according to the invention has very good strength properties, in particular a high transverse tensile strength of at least 2.5 N / mm 2 , preferably at most 3N / mm 2 , especially up to 4N / mm2 Preferably, the particleboard has a strength of 3000 N / mm 2 Up to 5000N / mm 2 , advantageously 3500 to 5000 N / mm 2 , particularly preferably 4000 to 5000 N / mm 2 of elastic modulus. Due to the good strength properties, the particleboards can be securely fixed using fewer fasteners (such as screws), because a single fastener can provide a better fixing force in the board. In addition, the higher transverse tensile strength allows for more intensive processing of the particleboards according to the invention, such as simple profiles milled into the side edges of the board. For example, at least one simple profile, such as a tongue-and-groove profile, can be processed on the narrow side of a particleboard, which orients the two intermeshing boards relative to each other not only in the vertical direction but also in the horizontal direction. The high bending strength of the particleboard (at least 35 N / mm 2 , preferably at least 40N / mm 2 ) are permitted for use as structural elements, such as wall reinforcements.
[0047] The invention also relates to the use of the above-described particleboard for construction purposes in interior and exterior areas. The particleboard according to the invention is characterized in that it can be used in a variety of ways due to minimal expansion, especially reduced thickness expansion in the area of the narrow faces. In interior construction, the particleboard can be used, for example, as a floor or as a floor layer, respectively with or without a coating. In this case, unlike, for example, non-waterproof floors or floor coverings, the particleboard can also be used in damp and wet spaces, especially because its narrow edges (which may have edge profiles and are generally more exposed to moisture) no longer expand significantly when exposed to water or high humidity and almost completely return to their original dimensions after drying.
[0048] Thus, for example, on known devices for producing wood panels, it is now possible to produce essentially non-expanding particle boards that are dimensionally and physically stable with respect to water or air humidity and have high strength values, which are not restricted to small sizes.
[0049] Of course, the particleboard according to the invention can also be used as wall or ceiling panels, as furniture panels and as structural panels, in particular in exterior constructions of wet and humid spaces or laboratories and technical spaces or workshops. In exterior constructions, the particleboard according to the invention is likewise suitable as structural panel, typically for example as facade paneling for exterior window panels, coverings including roof coverings and wall elements.
[0050] The particleboard according to the invention can be used, for example, for terrace structures or outdoor floors. In this way, the same floor or floor covering can be used for interior and adjacent exterior areas (terraces, balconies, facades, fire escapes, etc.) without causing any adverse effects. Preferably, the particleboard according to the invention can be used for structures in the exterior area, in particular furniture. For example, workshops, manufacturing halls or stables can be constructed without any problems with the particleboard according to the invention. In addition, due to its water resistance, the particleboard according to the invention can also be used, for example, for fire protection elements and components in shipbuilding, in particular when they are provided with or coated with fire protection substances.
[0051] The particleboard according to the invention is already suitable for the aforementioned applications in the uncoated state. After the coating, its suitability is even greater, since deformations due to the influence of moisture are further reduced. The particleboard can optionally be constructed as a panel and, if necessary, be provided with profiles on the edges. The profiles are preferably used to fasten two panels together. Two panels arranged side by side can also be connected butt-jointed as an alternative. They can be fixed, for example, by means of a double-sided adhesive tape, which is arranged in the side region of the joint between directly adjacent panels. It is also possible to glue directly adjacent panels or boards, preferably using a waterproof adhesive. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Embodiments of the present invention are described in detail below with reference to the accompanying drawings. Herein, it is shown:
[0053] FIG1 shows a flow chart of a method for manufacturing a particle board;
[0054] FIG2 shows a schematic perspective view of a particle board;
[0055] FIG3 shows a blank density distribution curve of an embodiment of a particle board according to the present invention (Invention 1), and
[0056] FIG. 4 shows the rough density distribution curve of a standard particle board of type P2 according to DIN EN 312. DETAILED DESCRIPTION
[0057] FIG. 1 shows a flow chart of a method for producing a particle board 1 according to FIG. 2 .
[0058] The method has the following steps:
[0059] - Provide chips (A)
[0060] - Provide adhesive (B)
[0061] - Apply adhesive (C)
[0062] - Formation of chip blocks (D)
[0063] - Pressed chip block (E)
[0064] To provide chips, wood-cellulose material, typically wood, such as round wood, new wood, old wood or residual wood, but also annual plants, such as straw or bagasse, is first processed in a single-stage or multi-stage chipping operation, such as in drum slicers and disc slicers and knife-ring flakers, into chips 7, 8. The chips 7, 8 are then dried, for example in a single-lane or three-lane drum dryer and graded, for example by means of a sieve, into fine chips 7 and coarse chips 8.
[0065] Use the mixture of thermosetting first component and thermoplastic second component as adhesive.Thermosetting component can be selected from amino plastics, such as melamine resin, methyl benzoate or urea-formaldehyde resin, or selected from phenolic resin, such as phenolic resin, which can be used separately or in the form of mixture.The second component is selected from MDI, eMDI, PMDI or polyurethane, which can also be used separately or in the form of mixture.Preferably, as in the embodiment, melamine resin is provided in combination with PMDI.After providing the cuttings and adhesive, then apply, for example, apply the adhesive to the cuttings.
[0066] In the known device for gluing chips, adhesive is sprayed by nozzle. The spray produced by the nozzle is deposited on the surface of the chips through the spraying, for example, by the spray consisting of adhesive falling from top to bottom. In addition to the adhesive, a hydrophobizing agent, for example paraffin or water wax, is applied to the chips with a share of 1% by weight calculated relative to absolutely dry wood. The high share of adhesive according to the present invention (here 25% by weight calculated relative to absolutely dry wood in the cover layer and 30% by weight calculated relative to absolutely dry wood in the middle layer) can be carried out in one or more channels according to the type, amount and combination of the components of the adhesive. If necessary, the chips can be dried after the components of the adhesive are applied. After the adhesive is applied completely, the chips are dried.
[0067] The adhesive is applied separately, for example, for the fine chips used to produce the cover layer and for the coarser chips used for the intermediate layer. For the fine chips, the composition of the adhesive can also be selected to be different from that for the coarser chips, for example, the proportion of the first thermoplastic component of the adhesive is smaller than that of the adhesive for the coarser chips. In this context, the adhesive is used together with the first component made of melamine resin and the second component made of PMDI in a ratio of 4:1 for the cover layer and in a ratio of 5:1 for the intermediate layer, wherein an average of 27.5% by weight is used, calculated relative to the absolutely dry wood, specifically divided into 25% by weight of adhesive calculated relative to the absolutely dry wood in the cover layer (25% and 50% of the board mass, respectively) and 30% by weight of adhesive calculated relative to the absolutely dry wood in the intermediate layer (also 50% of the board mass). Obviously, not only the proportion of the intermediate layer and the cover layer can be varied, but also the amount of adhesive used can be varied.
[0068] After the application of the binder and drying, the chips 7, 8 are applied to a known spreading device and spread into chip blocks, for example, for forming a lower cover layer 5, an intermediate layer 6 and an upper cover layer 5. The fine chips 7 for the cover layer 6 are deposited, for example, by means of known wind spreading methods. The coarser chips 8 are dropped for the intermediate layer 6, for example, by means of known throwing spreading methods.
[0069] Then, in a known continuously operating double belt hot press, at a temperature of 160° C. to 240° C. (here for example at 180° C.) and at a pressure of at most 5 N / mm 2 (Here it is 4.5N / mm 2 The three-layer chip block is pressed under a pressure of 6 s / mm to 20 s / mm (here 9.35 s / mm). Before and / or during the pressing of the chip block, a separating agent mixed with water, for example a liquid with different polymers, here containing silicone, is applied to the pressing plate or the pressing belt of the press to prevent adhesion. After pressing, the particle board is advantageously cooled at room temperature. In the known grinding device, the upper and lower sides 2, 3 of the particle board are then ground in two grinding processes respectively with a grinding device, the particle size of which is, for example, 50.
[0070] In a further step, the particleboard can be cut, milled and / or coated, for example painted, laminated or printed, for example, and then usually stacked and stored and / or prepared for transportation.
[0071] According to a preferred embodiment, as shown in FIG. 2 , the particleboard 1 produced by the above method has an upper side 2, an underside 3 and a narrow face 4 as well as an upper and lower cover layer (DS) 5 and an intermediate layer (MS) 6 arranged between the cover layers. The intermediate layer 6 has a substantially coarse chip 8 and the cover layer 5 has a substantially fine chip 7. The chips 7 and 8 are each embedded in an adhesive. The proportion of adhesive is greater than 15% by weight, calculated relative to the absolutely dry wood, and here the average is 27.5% by weight, calculated relative to the absolutely dry wood.
[0072] Particleboard 1 is compared with a standard particleboard of grade P2 (DIN EN 312: 2010), which is made of the same chip material and the same components of the adhesive, but has a significantly lower adhesive content in its middle layer and cover layer, wherein the cover layer of the standard particleboard P2 does not contain PMDI. In general, the PMDI content in the middle layer of the standard particleboard (0.1 to 0.6% by weight calculated relative to absolutely dry wood) is much smaller than in the case of the particleboard according to the invention (5% by weight calculated relative to absolutely dry wood). Figures 3 and 4 show the density distribution in a cross section of the particleboard. The unit of kg / m is plotted respectively for the position along the board thickness in mm. 3 In addition, in FIGS. 3 and 4 , the average density is shown by line H1, 85% of the average density is shown by line H2, the maximum density on the left (first cover layer) is shown by line V1, and the maximum density on the right (second cover layer) is shown by line V2. The particle board according to the invention has an average density of 850 kg / m3 to 950 kg / m3, here for example according to FIG. 3 897 kg / m3. 3 In comparison, standard particleboard P2 has a weight of 640 to 720 kg / m 3 The average density, here according to FIG. 4, is for example 707 kg / m 3 Furthermore, the particle board according to the invention has a relative humidity of about 1080 kg / m 3 The standard particle board P2 has a maximum density of about 850 kg / m in the cover layer (lines V1 and V2). 3 The maximum density.
[0073] Tables 1 and 2 below show the results of a comparison of two particleboards (Invention 1 and Standard) with the board thickness in mm as total value (before grinding) and in kg / m 3 The density is expressed in units of . The particleboards were evaluated according to transverse tensile strength (DIN EN 319), expansion (measured according to DIN EN 317) and edge expansion (measured according to DIN EN 13329) (see Table 2).
[0074] Furthermore, Table 1 shows the experimental results of two further embodiments of particleboard according to the present invention (Invention 2 and Invention 3). The second embodiment differs from the first embodiment in that the board thickness is 19 mm, the weight of the particleboard is 660 kg / m 3 The smaller target density is 490kg / m 3 The small chip usage and the resulting 130kg / m 3 In contrast, the difference between the third embodiment and the first embodiment under the same 8 mm plate thickness is that the third embodiment has a lower adhesive usage of 720 kg / m 3 The smaller target density is also 550 kg / m 3 The use of small chips and the resulting 150kg / m 3 Even these lighter particleboards still exhibit improved strength properties and improved water resistance or water resistance relative to the standard particleboard P2.
[0075] Table 1
[0076] Comparative test of a standard particle board and a particle board according to the invention:
[0077]
[0078] Table 2
[0079] Table 1 Comparative test of expansion and strength values of standard particleboard and particleboard according to the invention:
[0080]
[0081] *Cannot be measured
[0082] The particleboard according to the invention needs to be compacted more strongly than conventional standard particleboards. The adhesive coefficient is about 2 to 5 times higher than in the particleboard according to the prior art, in the example according to Table 1, about 3 times. The proportion of the second component of the adhesive is much higher than in standard particleboards; the second component is increased in excess of the increased use of the first component, by more than 10 times. The particleboard according to the invention has an expansion that is 10 times smaller than the original board (DIN EN 317) and a transverse tensile strength that is three times higher (DIN EN 319). In addition, the particleboard according to the invention has a modulus of elasticity that is more than 1.5 times higher and a flexural strength that is more than 1.5 times higher than the standard particleboard P2.
[0083] After coating the upper and lower sides, the edge expansion of the coated boards was measured. Only the narrow sides of the particleboards can still be touched by water, because the upper and lower sides of the board are sealed by the coating and water can no longer reach them. This test is of great significance for floor coverings, because usually the narrow sides of the floor cannot be sealed and are therefore exposed to water. Here, it was found that the particleboards according to the invention have significantly reduced edge expansion compared to known standard particleboards, while the edge expansion of standard particleboards is so high that it cannot be measured. It is worth noting that both standard particleboards and the particleboards according to the invention are produced on the same industrial production equipment.
[0084] Table 3 shows the formulation of a further embodiment of a particleboard according to the invention (Invention 4), which has a lower first thermosetting component portion (adhesion coefficient) of the adhesive in the cover layer and the intermediate layer than in the other embodiments. As the first thermosetting component, the adhesive in this embodiment comprises a melamine formaldehyde resin. The particleboard according to this embodiment is characterized by an elasticizing additive in the cover layer, for example styrene acrylate, as a result of which the particleboard according to the invention achieves better planarization. The components of the formulation are each expressed in % by weight calculated relative to the absolutely dry wood. In addition, according to this embodiment, for example water wax is added as a hydrophobizing agent (emulsion) and for example ammonium sulfate as a curing agent to the particleboard.
[0085] Table 3
[0086] The formulation of the particleboard according to the invention is:
[0087]
[0088]
[0089] Reference numerals list
[0090] 1 Particleboard
[0091] 2 upper side
[0092] 3 Lower side
[0093] 4 Narrow side
[0094] 5 Covering
[0095] 6 Middle Layer
[0096] 7 Fine chips
[0097] 8 Coarse chips
[0098] A provides chips
[0099] B Provide adhesive
[0100] C Apply adhesive
[0101] D Chip formation
[0102] E Pressed chip block
[0103] H1 Average density
[0104] H2 85% of the average density V1 Maximum density on the left V2 Maximum density on the right
Claims
1. A method for producing a particle board, comprising the following steps: - providing chips (7, 8) obtained from wood cutting, - providing at least one adhesive, - applying a binder to the chips (7, 8), wherein a binder content of at least 12% by weight, calculated on the absolutely dry chips, is applied to the chips (7, 8), - the formation of one or more layers of chip masses, and - pressing the chip mass in a hot press to produce a particle board (1), It is characterized in that - adding an elastomer or a thermoplastic as an elasticizing additive for improving the elastic properties of the particleboard, wherein The elasticizing additive is used as a solid in an amount of 1% to 7% by weight, based on the total amount of the particleboard (calculated on an absolute dry basis).
2. The method according to claim 1, wherein: The adhesive comprises at least a first component made of a thermosetting material and a second component made of a thermoplastic material, characterised in that the first component and the second component of the adhesive are applied to the chips (7, 8) in a ratio of first component to second component of 2:1 to 5:1, advantageously 3:1, preferably 4:1 or 5:
1.
3. The method according to claim 2, characterized in that Condensation resins, in particular aminoplasts, such as melamine-formaldehyde resins, benzoguanamine resins or urea-formaldehyde resins, or phenolic resins, such as phenol-formaldehyde resins, are used as the first thermosetting component of the adhesive, either alone and / or in a mixture.
4. The method according to claim 2 or 3, characterized in that: Technical-grade diphenylmethane diisocyanate PMID, diphenyl isocyanate MDI, or eMDI in emulsified form, or polyurethanes are used as the second thermoplastic component of the adhesive, respectively, alone and / or in the form of a mixture.
5. The method according to any one of the preceding claims, characterized in that One or more components of the adhesive are applied to the chips (7, 8) individually and / or in the form of a mixture.
6. The method according to any one of the preceding claims, characterized in that Acrylates, styrene acrylates or polyurethanes are used as elasticizing additives to increase the elasticity of the particleboard.
7. The method according to any one of the preceding claims, characterized in that The elasticizing additive is applied to the chips before or preferably after the application of the adhesive, in particular in addition to the application of the first component and the second component of the adhesive.
8. The method according to any one of the preceding claims, characterized in that A binder content of at least 15% by weight, calculated on the absolutely dry chips, preferably at least 17% by weight, calculated on the absolutely dry chips, particularly preferably at least 20% by weight, calculated on the absolutely dry chips, very particularly preferably at least 25% by weight, calculated on the absolutely dry chips, is applied to the chips (7, 8).
9. The method according to any one of the preceding claims, characterized in that The particle board (1) comprises at least a cover layer (5) and an intermediate layer (6), wherein the cover layer (5) and the intermediate layer (6) respectively have different adhesives and / or different adhesive compositions.
10. The method according to any one of the preceding claims, characterized in that The chips (7, 8) are pressed in a continuous press with a pressing factor of at least 6 s / mm to 20 s / mm, preferably 8 s / mm to 18 s / mm, particularly preferably 9 to 15 s / mm.
11. The method according to any one of the preceding claims, characterized in that The chips (7, 8) are pressed at a pressing pressure of 2 to 5 MPa, preferably 3 to 5 MPa, particularly preferably 3.5 to 5 MPa.
12. A method according to any one of the preceding claims, wherein: The particle board (1) is ground after pressing and / or after cooling, characterized in that grinding means with a grit size of at most 60, preferably at most 50, particularly preferably at most 40 are used.
13. A particle board, in particular a particle board produced by a method according to any one of the preceding claims, having chips obtained from wood cutting and a binder content of at least 12% calculated on absolutely dry wood, characterized in that - Addition of elastomers or thermoplastics as elastification additives, wherein: The elasticizing additive is used as a solid in an amount of 1% to 7% by weight, based on the total amount of the particleboard (calculated on an absolute dry basis).
14. The particle board according to claim 13, characterized in that The elasticizing additive is used as a solid in an amount of 2 to 7 wt %, preferably 2 to 6 wt %, particularly preferably 2.5 to 5.5 wt %, based on the total amount of the particleboard (calculated on an absolute dry basis).
15. The particle board according to claim 13 or 14, characterized in that It has a mass of 800 to 1000 kg / m 3 , preferably 850 to 950 kg / m 3 , particularly preferably 900 to 950 kg / m 3 The average density of .
16. The particle board according to any one of claims 13 to 15, characterized in that The maximum expansion of the particleboard is 4% of the initial thickness.
17. The particle board according to any one of claims 13 to 16, characterized in that It has 3000 to 5000 N / mm 2 , preferably 3500 to 5000 N / mm 2 , particularly preferably 4000 to 5000 N / mm 2 The elastic modulus.
18. Use of a particle board according to any one of claims 13 to 17 for construction purposes in the interior and exterior area, in particular for facade panels, exterior window panels, covers, roof coverings and wall elements and wet rooms.
Citation Information
Patent Citations
Method for producing wood fibre-plastics composite products
CN102470544A
Lignocellulose materials having good mechanical properties
EP2542625A1
Composite material manufactured from a binder system including waste powder coating powder
WO2008020768A1