Photocuring injectable biological ceramic-based composite hydrogel as well as preparation method and application thereof

By combining chitosan with zinc silicate, a photocured bioceramic-based hydrogel was prepared, which solved the problem of insufficient mechanical properties and antibacterial effects of existing hydrogels in chronic wound healing, and achieved efficient wound healing and tissue regeneration significantly accelerates the wound healing process by forming three-dimensional porous scaffolds and continuously releasing zinc and silicate ions.

CN118924944APending Publication Date: 2024-11-12CHENGDU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410999206.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing biohydrogels have problems with insufficient mechanical properties, micropore structure and antibacterial effects in promoting chronic wound healing, which is difficult to effectively accelerate wound healing.

Method used

By combining natural polymer chitosan with bioceramic zinc silicate, a photocurable injectable bioceramic matrix composite hydrogel was prepared. The mechanical properties and microporous structure were improved by dialysis and freeze-drying processes, and at 405 nm It solidifies rapidly in the band, forming a three-dimensional porous scaffold to promote tissue regeneration.

Benefits of technology

This hydrogel can directly reach the wound through injection, providing antibacterial and anti-inflammatory effects, promoting wound healing, improving cell growth environment, enhancing cell attachment sites, and synergistically exert hemostatic, proliferation and hemostatic by continuously releasing zinc ions and silicate ions The plastic effect significantly accelerates wound healing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118924944A_ABST
    Figure CN118924944A_ABST
Patent Text Reader

Abstract

The invention discloses a photocuring injectable bioceramic-based composite hydrogel and a preparation method and application thereof, and relates to the technical field of biomedical polymer materials, the method comprises the following steps: dissolving chitosan in an acetic acid solution, stirring, adding methacrylic anhydride, stirring in a water bath, then adjusting the pH value to be neutral, dialyzing and freeze-drying to obtain the photocuring injectable bioceramic-based composite hydrogel. The methylacryloylated chitosan is obtained; the preparation method comprises the following steps: dissolving methylacryloylated chitosan in a phosphate buffer solution, then adding phenyl (2, 4, 6-trimethylbenzoyl) lithium phosphate and zinc silicate, uniformly mixing, and carrying out vacuum defoaming. The invention further discloses the photocuring injectable biological ceramic based composite hydrogel and application thereof. The hydrogel is prepared by modifying natural polymer chitosan and then compounding with biological ceramic zinc silicate, so that the mechanical property, the microporous structure and the water content are improved, and the hydrogel has the effects of inhibiting bacteria, promoting tissue regeneration and accelerating wound healing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical polymer materials, and in particular to a photocurable injectable bioceramic-based composite hydrogel and a preparation method and application thereof. Background Art

[0002] Chronic wounds mostly include bedsores, limb ulcers and burns, which are often caused by physical or thermal damage that destroys the continuity of the epithelial lining of the skin or mucosa. They take a long time to repair and heal slowly, and are mainly divided into four stages: (1) hemostasis stage (just after injury); (2) inflammation stage (soon after injury and often swelling); (3) proliferation stage (end of inflammation stage, tissue and blood vessel regeneration); (4) remodeling stage (maturation and remodeling of new tissue). Each stage overlaps with each other and requires auxiliary drugs and other treatments. In recent years, biohydrogels have been developed, which often fit well with skin tissue and have good biocompatibility. They can also carry growth factors, drug systems, etc., directly reach the lesion site, reduce patients' pain and secondary infection of wounds, etc. Injectable hydrogels can be designed with microchannels through 3D printing technology and fine processing to construct a three-dimensional network structure of tissue scaffolds and accelerate tissue regeneration.

[0003] Chitosan is a natural macromolecular copolymer obtained by alkaline deacetylation. It can be metabolized by human lysozyme and has good biocompatibility, antibacterial and anti-inflammatory properties, and degradability. In the inorganic salt zinc silicate, silicate ions can promote the formation of new blood vessels. Among them, zinc ions participate in important processes such as protein synthesis, cell growth, division, and differentiation in life activities, and also participate in hormone metabolism. In damaged tissues, the zinc content will decrease, and appropriately increasing the zinc ion concentration can help promote wound healing. At the same time, zinc ions participate in the differentiation of epithelial tissues and have obvious antibacterial and anti-inflammatory effects. They can provide a more stable growth environment during wound healing and help improve the tolerance of fibroblasts to oxidative stress.

[0004] Therefore, providing an injectable hydrogel with high water content, mechanical properties and microporous structure, which can inhibit bacteria, promote tissue regeneration and accelerate wound healing is an urgent problem to be solved in the art. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a photocurable injectable bioceramic-based composite hydrogel and its preparation method and application. The hydrogel is prepared by modifying the natural polymer chitosan and then compounding it with the bioceramic zinc silicate, which improves the mechanical properties, microporous structure and water content, and has the effects of antibacterial, promoting tissue regeneration and accelerating wound healing.

[0006] The technical solution of the present invention to solve the above technical problem is as follows: a method for preparing a photocurable injectable bioceramic-based composite hydrogel is provided, comprising the following steps:

[0007] (1) dissolving chitosan in an acetic acid solution, adding methacrylic anhydride with stirring, stirring in a water bath, then adding a sodium hydroxide solution to adjust the pH to neutral, placing the chitosan in a dialysis bag, dialyzing it in deionized water, and then freeze-drying it to obtain methacrylylated chitosan;

[0008] (2) dissolving the methacryloyl chitosan obtained in step (1) in a phosphate buffer solution, then adding phenyl (2,4,6-trimethylbenzoyl) lithium phosphate and zinc silicate, mixing evenly, and removing bubbles in a vacuum to obtain a light-cured injectable bioceramic-based composite hydrogel.

[0009] Furthermore, in step (1), the concentration of the acetic acid solution is 1-3 vt%.

[0010] Furthermore, in step (1), stirring is performed in a water bath at 50-70° C. for 3-5 h.

[0011] Furthermore, in step (1), the molar ratio of the amino group of chitosan to methacrylic anhydride is 1:1-3.

[0012] Furthermore, in step (1), the molar ratio of the amino group of chitosan to methacrylic anhydride is 1:2.

[0013] The substitution degree of the finally obtained methacryloyl chitosan (CSMA) is 20%-50%. In improving the microenvironment of the composite material, the crosslinking strength, mechanical properties, porosity and water content are all well improved.

[0014] Furthermore, in step (1), the pH is adjusted to 7.0-7.4.

[0015] Furthermore, in step (1), the molecular weight cut-off of the dialysis bag is 12000Da.

[0016] Furthermore, in step (2), the mass volume ratio of methacryloyl chitosan, phenyl (2,4,6-trimethylbenzoyl) lithium phosphate, zinc silicate and phosphate buffer is 0.1-0.2 g: 0.01-0.03 g: 0.03-0.09 g: 10 mL.

[0017] Furthermore, in step (2), the mass volume ratio of methacryloyl chitosan, phenyl (2,4,6-trimethylbenzoyl) lithium phosphate, zinc silicate and phosphate buffer is 0.2g:0.025g:0.06g:10mL.

[0018] The present invention also provides a light-curable injectable bioceramic-based composite hydrogel prepared by the preparation method of the light-curable injectable bioceramic-based composite hydrogel.

[0019] The present invention also provides the use of the photocurable injectable bioceramic-based composite hydrogel in the preparation of medicines or reagents for promoting wound healing.

[0020] The present invention also provides the use of the photocurable injectable bioceramic-based composite hydrogel in the preparation of a hydrogel scaffold.

[0021] The present invention also provides the use of the photocurable injectable bioceramic-based composite hydrogel as a drug carrier.

[0022] The present invention has the following beneficial effects:

[0023] 1. The hydrogel of the present invention can be injected directly into the lesion, and the natural macromolecular chitosan is modified (such as Figure 1 The hydrogel forms a three-dimensional porous scaffold, which keeps the wound moist while providing channels for the exchange of substances and the migration of cells. The porous structure also provides attachment sites for cell growth. At the same time, inorganic salts also adhere to the material, which can increase its mechanical properties and achieve sustained release. At the same time, the hydrogel can also be used to prepare a hydrogel scaffold or as a drug carrier.

[0024] 2. During the whole process of wound healing, the hydrogel of the present invention can continuously release amino groups, zinc ions and silicate ions, and play a beneficial role at each stage. When the wound just begins, the amino groups of chitosan have a coagulation effect, which has a hemostatic effect, and chitosan and zinc ions work together to achieve antibacterial and anti-inflammatory effects; then chitosan and zinc silicate promote the proliferation and migration of cells at the wound, among which silicate ions are more conducive to the growth and expression of vascular cells. Through the synergistic effect of the two materials of modified chitosan and zinc silicate, antibacterial and anti-inflammatory effects are achieved and tissue growth is promoted, thereby maintaining the growth conditions of the wound and achieving the overall effect of promoting wound healing and remodeling. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of CSMA synthesis;

[0026] Figure 2 For CSMA 1 H NMR spectra;

[0027] Figure 3 ATR-FTIR graph of CSMA;

[0028] Figure 4 This is the result of measuring the water content of the hydrogel;

[0029] Figure 5 This is the 40% compression mechanical diagram of the hydrogel;

[0030] Figure 6 This is a diagram showing the injectability test results of the hydrogel;

[0031] Figure 7 This is a diagram of the HUVECs cell experiment results. DETAILED DESCRIPTION

[0032] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0033] Example 1

[0034] A photocurable injectable bioceramic-based composite hydrogel, the preparation method of which comprises the following steps:

[0035] (1) Chitosan (CS) was dissolved in 2vt% acetic acid solution, and methacrylic anhydride (MA) was added with stirring according to the molar ratio of amino group of chitosan to methacrylic anhydride being 1:2, and the mixture was stirred in a water bath at 60°C and 600 r / min for 4 h, and then sodium hydroxide solution was added to adjust the pH to neutral, and the mixture was placed in a 12000Da dialysis bag and dialyzed in deionized water, with the dialysate being changed twice a day for one week, and then freeze-dried to obtain methacrylylated chitosan (CSMA);

[0036] (2) 0.2 g of the methacryloyl chitosan obtained in step (1) was dissolved in 10 mL of phosphate buffered saline (PBS), and then 0.025 g of lithium phenyl (2,4,6-trimethylbenzoyl) phosphate (LAP) and 0.06 g of zinc silicate were added and mixed evenly, and vacuum degassing was performed to obtain a light-cured injectable bioceramic-based composite hydrogel.

[0037] Example 2

[0038] A photocurable injectable bioceramic-based composite hydrogel, the preparation method of which comprises the following steps:

[0039] (1) Chitosan was dissolved in 1vt% acetic acid solution, and methacrylic anhydride was added with stirring according to the molar ratio of amino group of chitosan to methacrylic anhydride of 1:1, and stirred in a water bath at 50°C and 400 r / min for 3 h, and then sodium hydroxide solution was added to adjust the pH to neutral, and the mixture was placed in a 12000Da dialysis bag and dialyzed in deionized water, with the dialysate changed twice a day for one week, and then freeze-dried to obtain methacrylylated chitosan;

[0040] (2) 0.1 g of the methacryloyl chitosan obtained in step (1) was dissolved in 10 mL of phosphate buffer, and then 0.01 g of phenyl (2,4,6-trimethylbenzoyl) lithium phosphate and 0.03 g of zinc silicate were added and mixed evenly, and vacuum degassing was performed to obtain a light-cured injectable bioceramic-based composite hydrogel.

[0041] Example 3

[0042] A photocurable injectable bioceramic-based composite hydrogel, the preparation method of which comprises the following steps:

[0043] (1) Chitosan was dissolved in 3vt% acetic acid solution, and methacrylic anhydride was added with stirring according to the molar ratio of amino group of chitosan to methacrylic anhydride of 1:3, and stirred in a water bath at 70°C and 800 r / min for 5 h, and then sodium hydroxide solution was added to adjust the pH to neutral, and the chitosan was placed in a 12000Da dialysis bag and dialyzed in deionized water, with the dialysate changed twice a day for one week, and then freeze-dried to obtain methacrylylated chitosan;

[0044] (2) 0.2 g of the methacryloyl chitosan obtained in step (1) was dissolved in 10 mL of phosphate buffer, and then 0.03 g of phenyl (2,4,6-trimethylbenzoyl) lithium phosphate and 0.09 g of zinc silicate were added and mixed evenly, and vacuum degassing was performed to obtain a light-cured injectable bioceramic-based composite hydrogel.

[0045] Example 4

[0046] A photocurable injectable bioceramic-based composite hydrogel, the preparation method of which comprises the following steps:

[0047] (1) Chitosan was dissolved in 2vt% acetic acid solution, and methacrylic anhydride was added with stirring according to the molar ratio of amino group of chitosan to methacrylic anhydride of 1:2, and stirred in a water bath at 60°C and 600 r / min for 4 h, and then sodium hydroxide solution was added to adjust the pH to neutral, and the chitosan was placed in a 12000Da dialysis bag and dialyzed in deionized water, with the dialysate changed twice a day for one week, and then freeze-dried to obtain methacrylylated chitosan;

[0048] (2) 0.15 g of the methacryloyl chitosan obtained in step (1) was dissolved in 10 mL of phosphate buffer, and then 0.02 g of phenyl (2,4,6-trimethylbenzoyl) lithium phosphate and 0.06 g of zinc silicate were added and mixed evenly, and vacuum degassing was performed to obtain a light-cured injectable bioceramic-based composite hydrogel.

[0049] Test Example 1

[0050] (1) Chitosan (CS) and methacrylylated chitosan (CSMA) prepared in Example 1 were subjected to 1H NMR and ATR-FTIR tests, the results are as follows Figure 2 and Figure 3 shown.

[0051] according to Figure 2 The peak area in the spectrum was calculated using the software MestReNova. The degree of methacrylation was determined by the ratio of the average proton peak area of ​​the methacrylamide group (δ = 5.2-5.8 ppm) to the average proton area of ​​the CS glucosamine ring (δ = 2.6-4.0 ppm). The degree of substitution after modified grafting was calculated using the formula:

[0052] Depend on Figure 3 It can be seen that the spectrum shows 1025-1151cm -1 The characteristic absorption band at 2859 cm-1 belongs to the amine CN extension of CS. -1 and 2925cm -1 The intensity of the absorption band at 1637 cm-1 increases significantly, corresponding to the alkyl CH stretching of CS and methacrylate groups. -1 、1540cm -1 and 1315cm -1 Several new peaks appeared at 400 nm, which were due to the new conformation of amide, and should be attributed to amide type I (C=O stretching), type II (NH deformation and CN stretching) and type III. The results of this spectrum further verified the successful methacrylation of CS.

[0053] (2) The hydrogel prepared in Example 1 was subjected to an extrusion experiment using a 5 mL syringe. The results are as follows: Figure 4 shown.

[0054] Depend on Figure 4 It can be seen that the hydrogel has good extrusion fluidity and will not cause problems such as clogging.

[0055] Test Example 2

[0056] Referring to Example 1, light-curable injectable bioceramic-based composite hydrogels with different zinc silicate contents (0 g, 0.03 g, 0.06 g, and 0.09 g) were prepared. The hydrogel was added to a cylindrical mold with a diameter of 10 mm and irradiated under 405 nm ultraviolet light for 10 seconds for curing. The cured model was then taken out for testing.

[0057] (1) Carefully wipe the surface water of the solidified hydrogel with filter paper, then weigh and record it, and then weigh it again after freeze-drying to obtain the mass difference. The water content result is as follows: Figure 5 shown.

[0058] Depend on Figure 5 It can be seen that the hydrogels in each ratio have a high water content and can maintain a certain humidity at the wound.

[0059] (2) Place the cured model into a compression test machine and perform a 40% compression test. The results are as follows: Figure 6 shown.

[0060] At 40% strain, the hydrogel remains intact. Figure 6 It can be seen that the hydrogel has good mechanical strength. At the same time, as the content of zinc silicate increases, it is mixed inside the hydrogel, attached or embedded in the three-dimensional network, so that the overall mechanical properties of the hydrogel are also increased.

[0061] (3) The solidified models of each group were sterilized by immersion in alcohol and UV irradiation, and then immersed in complete culture medium for two days. The leaching solution was filtered with a 0.22 μm filter membrane, and the filtered leaching solution and umbilical vein endothelial cells (HUVECs) were used for cell experiments. The results are as follows: Figure 7 As shown, A is a proliferation experiment result diagram, B is a scratch healing experiment result diagram, C is a scratch healing area comparison diagram, and D is a cell proliferation OD value comparison diagram.

[0062] Depend on Figure 7 It can be seen that the hydrogels with different ratios all showed good biocompatibility, proliferation rate and scratch healing effect, among which the CSMA / ZS-0.6 group was better.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a photocurable injectable bioceramic-based composite hydrogel, It is characterized in that The following steps are involved: (1) dissolving chitosan in an acetic acid solution, adding methacrylic anhydride with stirring, stirring in a water bath, then adding a sodium hydroxide solution to adjust the pH to neutral, placing the chitosan in a dialysis bag, dialyzing it in deionized water, and then freeze-drying it to obtain methacrylylated chitosan; (2) dissolving the methacryloyl chitosan obtained in step (1) in a phosphate buffer solution, then adding phenyl (2,4,6-trimethylbenzoyl) lithium phosphate and zinc silicate, mixing evenly, and removing bubbles in a vacuum to obtain a light-cured injectable bioceramic-based composite hydrogel.

2. The method for preparing the photocurable injectable bioceramic-based composite hydrogel according to claim 1, It is characterized in that In step (1), the concentration of the acetic acid solution is 1-3 vt%.

3. The method for preparing the photocurable injectable bioceramic-based composite hydrogel according to claim 1, It is characterized in that In step (1), stir in a water bath at 50-70°C for 3-5 hours.

4. The method for preparing the photocurable injectable bioceramic-based composite hydrogel according to claim 1, It is characterized in that In step (1), the molar ratio of the amino group of the chitosan to methacrylic anhydride is 1:1-3.

5. The method for preparing the photocurable injectable bioceramic-based composite hydrogel according to claim 1, It is characterized in that In step (1), the molecular weight cut-off of the dialysis bag is 12000Da.

6. The method for preparing the photocurable injectable bioceramic-based composite hydrogel according to claim 1, It is characterized in that In step (2), the mass volume ratio of the methacryloyl chitosan, phenyl (2,4,6-trimethylbenzoyl) lithium phosphate, zinc silicate and phosphate buffer is 0.1-0.2 g: 0.01-0.03 g: 0.03-0.09 g: 10 mL.

7. The photocurable injectable bioceramic-based composite hydrogel prepared by the method for preparing the photocurable injectable bioceramic-based composite hydrogel according to any one of claims 1 to 6.

8. Use of the photocurable injectable bioceramic-based composite hydrogel according to claim 7 in the preparation of medicines or reagents for promoting wound healing.

9. Use of the photocurable injectable bioceramic-based composite hydrogel according to claim 7 in the preparation of a hydrogel scaffold.

10. Use of the photocurable injectable bioceramic-based composite hydrogel according to claim 7 as a drug carrier.

Citation Information

Cited By

  • High-toughness antibacterial hemostatic chitosan hydrogel dressing and preparation method thereof

    CN119680004A