Pipe flow mechanism of gas-liquid two-phase flow guide type fire monitor and manufacturing method of pipe flow mechanism

By using high-hardness and high-temperature stable materials combinations in gas-liquid two-phase diversion fire guns, the hollow funnel-like structure and high-temperature sintering process are designed, which solves the problems of diversion tube wear and thermal fatigue, and improves the resistance of diversion tubes Wear and thermal shock performance meet the needs of efficient fire extinguishing in complex fire environments.

CN118925175APending Publication Date: 2024-11-12CHINA POWER ENG CONSULTING GRP CORP EAST CHINA ELECTRIC POWER DESIGN INST +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411102746.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing metal diversion pipes are prone to wear, thermal fatigue and cracks in complex fire environments, resulting in reduced performance and shortened service life, making it difficult to meet the needs of efficient fire extinguishing.

Method used

The gas-liquid two-phase diversion fire-fighting gun barrel flow mechanism adopts a hollow funnel-like structure. Through the combination of monoclinic zirconia, cerium oxide, quartz powder, magnesium oxide and sodium aluminum silicate aluminum phosphate, combined with high-temperature kiln sintering and The use of magnetic separation equipment forms a flow guide tube with high hardness and high temperature stability.

Benefits of technology

The deflector is achieved in the long-term use of wear and stability in high temperature environments, significantly improves thermal shock performance and fire extinguishing efficiency, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925175A_ABST
    Figure CN118925175A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fire fighting equipment, and discloses a gas-liquid two-phase flow guide type fire monitor pipe flow mechanism which comprises a pipe body, the pipe body is of a hollow funnel-shaped structure, a necking-down section used for disturbing gas and liquid is arranged at the upward position of the pipe wall of the pipe body, the necking-down section is of an annular structure, and the section of the necking-down section is of a right trapezoid structure; and the gas-liquid is guided to be gathered at the pipe orifice. Through high hardness and good wear resistance of monoclinic zirconium oxide and cerium oxide, a firm structure is formed, so that the flow guide pipe can effectively resist wear in long-term use, and meanwhile, due to high melting point and low thermal expansion coefficient of magnesium oxide, the flow guide pipe is not easy to deform and crack in a high-temperature environment, so that the flow guide pipe is more durable. The pipe flow mechanism of the fire monitor can better adapt to a fire scene environment, and can effectively relieve thermal stress, so that the pipe flow mechanism of the fire monitor can still keep excellent performance when being continuously used in the fire scene, and the fire extinguishing efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fire fighting equipment, in particular to a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire fighting cannon and a manufacturing method thereof. Background Art

[0002] The gas-liquid two-phase diversion fire monitor is an important equipment widely used in the field of fire fighting. It effectively extinguishes fires by spraying a gas-liquid two-phase mixture. The diversion pipe flow structure is an important component of the fire monitor, and its performance directly affects the fire extinguishing effect and service life of the fire monitor.

[0003] With the development of fire protection technology and the complexity of the application environment, the performance requirements for the guide tube are getting higher and higher. The existing metal guide tube can no longer meet the needs of efficient fire extinguishing in complex fire environments. The high-pressure water flow will continuously flush the guide tube flow mechanism, causing serious wear on the inner wall of the tube, resulting in performance degradation and shortened service life. In addition, the metal guide tube is prone to thermal fatigue and cracks under rapid temperature changes, affecting its safety and stability. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor and a manufacturing method thereof, which solves the problems of severe internal wear of the pipe wall and poor thermal shock performance of the existing pipe flow mechanism after long-term operation.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: a pipe flow mechanism of a gas-liquid two-phase diversion fire cannon, including a pipe body, the pipe body is a hollow funnel-shaped structure, and a necking section for disturbing gas and liquid is provided at the upward position of its pipe wall, the necking section is an annular structure and its cross-section is a right-angled trapezoidal structure, which is used to guide the gas and liquid to converge at the pipe mouth.

[0006] A method for manufacturing a pipe flow mechanism based on the pipe flow mechanism of the gas-liquid two-phase flow-guiding fire monitor comprises the following steps:

[0007] S1. Take the following raw materials by mass: 50-60 parts of monoclinic zirconium oxide, 10-15 parts of cerium oxide, 20-25 parts of quartz powder, 10-15 parts of slaked lime, 5-10 parts of Portland cement, 2-5 parts of magnesium oxide, and 14-21 parts of inorganic ceramic binder;

[0008] S2, adding the above raw materials except the inorganic ceramic binder into a ball mill and mixing them evenly, sieving, then adding the inorganic ceramic binder, and then adding into a mixer and mixing evenly;

[0009] S3, press the mixed powder into blocks by a hydraulic press, put it into an oven for drying, and then put it into a high-temperature kiln and burn it to 800℃~1000℃ and maintain the temperature for 1.5h~3h, then close the kiln and wait for it to cool naturally to room temperature before taking it out of the kiln;

[0010] S4. The product after being taken out of the furnace is crushed, iron-removed and screened to obtain a mixed powder with a particle size of 100nm to 200nm, and an inorganic ceramic binder is added and mixed. After being placed for 6h to 8h, it is dry-pressed into shape by an upper press, and the moisture is dried. It is placed in an electric kiln and fired at 1600℃ to 1700℃, kept warm for 5h to 8h, and naturally cooled out of the furnace to obtain a guide tube.

[0011] Preferably, the flow guide tube is funnel-shaped, which facilitates the smooth flow of the gas-liquid two-phase mixture;

[0012] The funnel-shaped design is produced by precision moulding.

[0013] Preferably, the inorganic ceramic binder is a combination of sodium silicate and aluminum phosphate;

[0014] The concentration of the inorganic ceramic binder must be controlled within the range of 13% to 18% during mixing.

[0015] Preferably, when the mixed powder is crushed and iron removed and screened, a magnetic separation device with a magnetic field strength of 3000 to 5000 Gauss is used;

[0016] Meanwhile, the operating temperature range of the magnetic separation equipment is set to 0°C to 40°C, the feed rate is set to 1t / h and the separation time is set to 15 to 26min.

[0017] Preferably, after the powder is dry-pressed by the upper press, it needs to be subjected to a secondary drying treatment at a temperature of 110° C. for 1.5 hours;

[0018] The secondary drying process must be carried out in a closed environment to prevent the influence of moisture.

[0019] Preferably, the temperature increase rate of the high temperature kiln is controlled at 100°C / h to prevent thermal stress of the material;

[0020] The temperature increase process must be carried out under the protection of inert gas.

[0021] Preferably, the cooling process needs to adopt a staged cooling method;

[0022] The cooling rate of the high temperature kiln is controlled at 50°C / h to avoid thermal cracks in the draft tube.

[0023] Preferably, the powder is screened by a laser particle size analyzer to obtain a particle size range of 100 nm to 200 nm;

[0024] The laser power of the laser particle size analyzer was set to 10-50 mW and 2200-4500 times / sec.

[0025] Preferably, the inner wall of the guide tube is polished to reduce the adhesion of liquid on the inner wall of the guide tube, and the inner wall polishing adopts electrolytic polishing technology;

[0026] The outer wall of the guide tube is polished by polishing equipment.

[0027] The present invention provides a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor and a manufacturing method thereof. It has the following beneficial effects:

[0028] 1. The present invention forms a strong structure through the high hardness and good wear resistance of monoclinic zirconium oxide and cerium oxide, so that the guide tube can effectively resist wear during long-term use. At the same time, the magnesium oxide and quartz powder used provide structural stability at high temperatures. In particular, the high melting point and low thermal expansion coefficient of magnesium oxide make the guide tube less likely to deform and crack in a high temperature environment, and can better adapt to the use in a fire scene environment.

[0029] 2. The pipe flow mechanism manufactured by the present invention shows better thermal shock performance. The ceramic binder formed by sodium silicate and aluminum phosphate remains stable at high temperatures, and the thermal expansion coefficients of cerium oxide and quartz powder are low, which can effectively relieve thermal stress, so that the pipe flow mechanism of the fire monitor can still maintain excellent performance when continuously used in the fire scene, thereby improving the efficiency of fire extinguishing. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a cross-sectional view of the present invention.

[0031] Among them, 1. tube body; 2. necking section. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Embodiment 1:

[0034] Please see attached Figure 1 The embodiment of the present invention provides a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor and a manufacturing method thereof, including:

[0035] Raw material ratio:

[0036] Monoclinic zirconium oxide: 55 parts

[0037] Cerium oxide: 12 parts

[0038] Quartz powder: 22 parts

[0039] Hydrated lime: 12 parts

[0040] Portland cement: 8 parts

[0041] Magnesium oxide: 4 parts

[0042] Inorganic ceramic binder: 15 parts

[0043] Mixing steps:

[0044] Add the raw materials except the inorganic ceramic binder into a ball mill, mix evenly, and sieve.

[0045] Add inorganic ceramic binder and mix well in a mixer.

[0046] Pressing and sintering:

[0047] The mixed powder is pressed into blocks by a hydraulic press and placed in an oven for drying.

[0048] Put it into a high-temperature kiln and burn it to 900℃, keep it for 2 hours, then close the kiln and wait for it to cool naturally to room temperature.

[0049] Powder handling:

[0050] The product after being fired is crushed, iron-removed and screened to obtain a mixed powder with a particle size of 150nm.

[0051] Add inorganic ceramic binder and mix, let stand for 7 hours, then dry-press into shape using an upper press to dry out moisture.

[0052] Final sintering:

[0053] Put it into an electric kiln and burn it to 1650℃, keep it warm for 6 hours, cool it naturally and take it out of the kiln to get the guide tube.

[0054] Embodiment 2:

[0055] Please see attached Figure 1 The embodiment of the present invention provides a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor and a manufacturing method thereof, including:

[0056] Raw material ratio:

[0057] Monoclinic zirconium oxide: 60 parts

[0058] Cerium oxide: 15 parts

[0059] Quartz powder: 25 parts

[0060] Quicklime: 10 parts

[0061] Portland cement: 10 parts

[0062] Magnesium oxide: 5 parts

[0063] Inorganic ceramic binder: 18 parts

[0064] Mixing steps:

[0065] Add the raw materials except the inorganic ceramic binder into a ball mill, mix evenly, and sieve.

[0066] Add inorganic ceramic binder and mix well in a mixer.

[0067] Pressing and sintering:

[0068] The mixed powder is pressed into blocks by a hydraulic press and placed in an oven for drying.

[0069] Put it into a high-temperature kiln and burn it to 950℃, keep it for 1.5 hours, then close the kiln and wait for it to cool naturally to room temperature.

[0070] Powder handling:

[0071] The product after being fired is crushed, iron-removed and screened to obtain a mixed powder with a particle size of 120 nm.

[0072] Add inorganic ceramic binder and mix, place for 8 hours, then dry-press into shape using an upper press to dry out moisture.

[0073] Final sintering:

[0074] Put it into an electric kiln and burn it to 1700℃, keep it warm for 5 hours, cool it naturally and take it out of the kiln to get the guide tube.

[0075] Embodiment 3:

[0076] Please see attached Figure 1 The embodiment of the present invention provides a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor and a manufacturing method thereof, including:

[0077] Raw material ratio:

[0078] Monoclinic zirconium oxide: 50 parts

[0079] Cerium oxide: 10 parts

[0080] Quartz powder: 20 parts

[0081] Quicklime: 15 parts

[0082] Portland cement: 5 parts

[0083] Magnesium oxide: 2 parts

[0084] Inorganic ceramic binder: 14 parts

[0085] Mixing steps:

[0086] Add the raw materials except the inorganic ceramic binder into a ball mill, mix evenly, and sieve.

[0087] Add inorganic ceramic binder and mix well in a mixer.

[0088] Pressing and sintering:

[0089] The mixed powder is pressed into blocks by a hydraulic press and placed in an oven for drying.

[0090] Put it into a high temperature kiln and burn it to 850℃, keep it for 3 hours, then close the kiln and wait for it to cool naturally to room temperature.

[0091] Powder handling:

[0092] The product after being fired is crushed, iron-removed and screened to obtain a mixed powder with a particle size of 200 nm.

[0093] Add inorganic ceramic binder and mix, let stand for 6 hours, then dry-press and form by upper press to dry out moisture.

[0094] Final sintering:

[0095] Put it into an electric kiln and burn it to 1600℃, keep it warm for 8 hours, cool it naturally and take it out of the kiln to get the guide tube.

[0096] Embodiment 4:

[0097] Please see attached Figure 1 The embodiment of the present invention provides a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor and a manufacturing method thereof, including:

[0098] Raw material ratio:

[0099] Monoclinic zirconium oxide: 57 parts

[0100] Cerium oxide: 13 parts

[0101] Quartz powder: 23 parts

[0102] Quicklime: 13 parts

[0103] Portland cement: 7 parts

[0104] Magnesium oxide: 3 parts

[0105] Inorganic ceramic binder: 16 parts

[0106] Mixing steps:

[0107] Add the raw materials except the inorganic ceramic binder into a ball mill, mix evenly, and sieve.

[0108] Add inorganic ceramic binder and mix well in a mixer.

[0109] Pressing and sintering:

[0110] The mixed powder is pressed into blocks by a hydraulic press and placed in an oven for drying.

[0111] Put it into a high-temperature kiln and burn it to 875℃, keep it for 2.5 hours, then close the kiln and wait for it to cool naturally to room temperature.

[0112] Powder handling:

[0113] The product after being fired is crushed, iron-removed and screened to obtain a mixed powder with a particle size of 180 nm.

[0114] Add inorganic ceramic binder and mix, let stand for 7 hours, then dry-press into shape using an upper press to dry out moisture.

[0115] Final sintering:

[0116] The product is placed in an electric kiln and fired to 1675°C, kept at this temperature for 6.5 hours, cooled naturally and taken out of the kiln to obtain a guide tube.

[0117] Embodiment 5:

[0118] Please see attached Figure 1 The embodiment of the present invention provides a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor and a manufacturing method thereof, including:

[0119] Raw material ratio:

[0120] Monoclinic zirconium oxide: 53 parts

[0121] Cerium oxide: 11 parts

[0122] Quartz powder: 21 parts

[0123] Quicklime: 11 parts

[0124] Portland cement: 6 parts

[0125] Magnesium oxide: 4 parts

[0126] Inorganic ceramic binder: 17 parts

[0127] Mixing steps:

[0128] Add the raw materials except the inorganic ceramic binder into a ball mill, mix evenly, and sieve.

[0129] Add inorganic ceramic binder and mix well in a mixer.

[0130] Pressing and sintering:

[0131] The mixed powder is pressed into blocks by a hydraulic press and placed in an oven for drying.

[0132] Place it in a high temperature kiln and heat it to 925°C, keep it for 1.75 hours, then close the kiln and wait for it to cool naturally to room temperature.

[0133] Powder handling:

[0134] The product after being fired is crushed, iron-removed and screened to obtain a mixed powder with a particle size of 140 nm.

[0135] Inorganic ceramic binder is added to the mixture, and after being left for 6.5 hours, the mixture is dry-pressed into a shape by an upper press to dry out the moisture.

[0136] Final sintering:

[0137] The product is placed in an electric kiln and fired at 1625°C, kept at this temperature for 5.5 hours, cooled naturally and taken out of the kiln to obtain a guide tube.

[0138] Comparative experiment:

[0139] Experiment 1: Wear resistance test

[0140] Purpose: To test the wear resistance of the flow guide tube under abrasive conditions.

[0141] method:

[0142] Using a wear tester, wear tests were performed on the flow guide tubes manufactured in each embodiment and the conventional method.

[0143] Record the wear amount (mg).

[0144] Comparison parameters:

[0145] Wear amount (mg)

[0146] Experiment 2: High temperature resistance test

[0147] Purpose: To test the structural stability of the flow guide tube in high temperature environment.

[0148] method:

[0149] The flow guide tube manufactured in each embodiment and the conventional method was placed in a high temperature furnace and kept at 1700° C. for 2 hours.

[0150] The structural change of the flow guide tube (mm) was recorded.

[0151] Comparison parameters:

[0152] Structural change (mm)

[0153] Experiment 3: Diversion efficiency test

[0154] Purpose: To test the diversion efficiency of the diversion tube in the fire monitor simulation experiment.

[0155] method:

[0156] The flow guide pipe manufactured by each embodiment and the conventional method is installed on a fire monitor simulation device.

[0157] Test its flow rate (L / min) within a fixed time.

[0158] Comparison parameters:

[0159] Flow efficiency (L / min)

[0160] Experiment 4: Corrosion resistance test

[0161] Purpose: To test the corrosion resistance of the flow guide tube in a corrosive environment.

[0162] method:

[0163] The flow guide tube manufactured in each example and the conventional method was immersed in a corrosive solution (such as 10% HCl solution) for 72 hours.

[0164] Observe and record changes in the surface and structure of the flow tube.

[0165] Comparison parameters:

[0166] Corrosion depth (mm)

[0167] Surface changes (picture record)

[0168] Experiment 5: Mechanical Strength Test

[0169] Purpose: To test the mechanical strength of the flow guide tube, including compressive strength and bending strength.

[0170] method:

[0171] The compressive strength and flexural strength tests were performed on the flow guide tubes manufactured in each embodiment and the conventional method using a material testing machine.

[0172] The compressive strength (MPa) and flexural strength (MPa) were recorded.

[0173] Comparison parameters:

[0174] Compressive strength(MPa)

[0175] Flexural strength(MPa)

[0176] Experiment 6: Thermal Shock Test

[0177] Purpose: To test the thermal shock performance of the draft tube in rapid temperature changes.

[0178] method:

[0179] The flow guide tubes manufactured in each embodiment and the conventional method were repeatedly and alternately immersed in water at 1000° C. and room temperature for 20 cycles.

[0180] Observe and record cracks and damage on the guide tube.

[0181] Comparison parameters:

[0182] Number of cracks

[0183] Damaged area (mm 2 )

[0184] The experimental results are shown in Table 1 below:

[0185]

[0186]

[0187] Table 1

[0188] in conclusion:

[0189] Wear resistance: The flow guide tube manufactured by the present invention shows significantly lower wear in the wear test, indicating that it has excellent wear resistance. The reason is that the monoclinic zirconium oxide and cerium oxide have high hardness and good wear resistance, and these materials form a solid structure, so that the flow guide tube can effectively resist wear in long-term use.

[0190] High temperature resistance: The flow guide tube manufactured by the present invention has smaller structural changes under high temperature conditions and shows better high temperature stability. The magnesium oxide and quartz powder used in the formula provide structural stability under high temperature, especially the high melting point and low thermal expansion coefficient of magnesium oxide, which makes the flow guide tube less likely to deform and crack under high temperature environment, and can better adapt to the use in fire scene environment.

[0191] Thermal shock performance: The number of cracks and the damaged area of ​​the flow guide tube produced by the present invention in the thermal shock test are significantly less than those of the traditional method, showing better thermal shock performance. The ceramic binder formed by sodium silicate and aluminum phosphate remains stable at high temperatures, and the thermal expansion coefficients of cerium oxide and quartz powder are low, which can effectively relieve thermal stress.

[0192] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor, comprising a pipe body (1), characterized in that: The tube body (1) is a hollow funnel-shaped structure, and a constricted section (2) for disturbing gas and liquid is provided at an upward position of the tube wall. The constricted section (2) is an annular structure and its cross section is a right-angled trapezoidal structure, and is used to guide gas and liquid to converge at the tube mouth.

2. A method for manufacturing a pipe flow mechanism of a gas-liquid two-phase flow-guiding fire monitor according to claim 1, characterized in that: The following steps are involved: S1. Take the following raw materials by mass: 50-60 parts of monoclinic zirconium oxide, 10-15 parts of cerium oxide, 20-25 parts of quartz powder, 10-15 parts of slaked lime, 5-10 parts of Portland cement, 2-5 parts of magnesium oxide, and 14-21 parts of inorganic ceramic binder; S2, adding the above raw materials except the inorganic ceramic binder into a ball mill and mixing them evenly, sieving, then adding the inorganic ceramic binder, and then adding into a mixer and mixing evenly; S3, press the mixed powder into blocks by a hydraulic press, put it into an oven for drying, and then put it into a high-temperature kiln and burn it to 800℃~1000℃ and maintain the temperature for 1.5h~3h, then close the kiln and wait for it to cool naturally to room temperature before taking it out of the kiln; S4. The product after being taken out of the furnace is crushed, iron-removed and screened to obtain a mixed powder with a particle size of 100nm to 200nm, and an inorganic ceramic binder is added and mixed. After being placed for 6h to 8h, it is dry-pressed into shape by an upper press, and the moisture is dried. It is placed in an electric kiln and fired at 1600℃ to 1700℃, kept warm for 5h to 8h, and naturally cooled out of the furnace to obtain a guide tube.

3. A method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: The draft tube is funnel-shaped, which helps the smooth flow of the gas-liquid two-phase mixture; The funnel-shaped design is produced by precision moulding.

4. A method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: The inorganic ceramic binder is a combination of sodium silicate and aluminum phosphate; The concentration of the inorganic ceramic binder must be controlled within the range of 13% to 18% during mixing.

5. The method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: When the mixed powder is crushed and iron removed and screened, a magnetic separation device with a magnetic field strength of 3000 to 5000 gauss is used; Meanwhile, the operating temperature range of the magnetic separation equipment is set to 0°C to 40°C, the feed rate is set to 1t / h and the separation time is set to 15 to 26min.

6. A method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: After the powder is dry-pressed by the upper press, it needs to be dried for a second time at a temperature of 110°C for 1.5 hours; The secondary drying process must be carried out in a closed environment to prevent the influence of moisture.

7. A method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: The temperature increase rate of the high temperature kiln is controlled at 100°C / h to prevent thermal stress of the material; The temperature increase process must be carried out under the protection of inert gas.

8. A method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: The cooling process needs to adopt a staged cooling method; The cooling rate of the high temperature kiln is controlled at 50°C / h to avoid thermal cracks in the draft tube.

9. A method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: The powder is screened by a laser particle size analyzer to obtain a particle size range of 100nm to 200nm; The laser power of the laser particle size analyzer was set to 10-50 mW and 2200-4500 times / sec.

10. A method for manufacturing a pipe flow mechanism according to claim 2, characterized in that: The inner wall of the guide tube is polished to reduce the adhesion of liquid on the inner wall of the guide tube, and the inner wall polishing adopts electrolytic polishing technology; The outer wall of the guide tube is polished by polishing equipment.

Citation Information

Patent Citations

  • Calcium barium zirconate titanate base piezoceramics and preparation method thereof

    CN101648807A