Lithium slag-based ion sieve adsorbent, preparation method thereof and lithium ion adsorption column

Through the preparation and treatment of lithium mica smelting slag, lithium slag-based ion sieve adsorbent is made and filled into the lithium ion adsorption column, which solves the problems of poor selectivity and low recycling rate of lithium ion extraction in salt lake brine, and achieves high efficiency , economical lithium ion extraction and resource recycling.

CN118925661APending Publication Date: 2024-11-12JIANGXI JIULING LITHIUM CO LTD

Patent Information

Application Number
CN202411136734.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional lithium extraction technology has poor selectivity, low recycling rate and high cost from salt lake brine, making it difficult to efficiently extract lithium ions.

Method used

Lithium mica smelting slag is used as raw material, and the lithium slag-based ion sieve adsorbent is prepared by washing, acid solution replacement and metaaluminate solution treatment, and fill it into a lithium ion adsorption column, using its high selectivity and circulation Lithium ions are extracted in a regenerative manner.

Benefits of technology

High selective extraction and recycling of lithium ions are achieved, production costs are reduced, the utilization efficiency of lithium resources is improved, and excellent adsorption performance is shown in complex ion environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925661A_ABST
    Figure CN118925661A_ABST
Patent Text Reader

Abstract

The invention provides a lithium slag-based ion sieve adsorbent, a preparation method thereof and a lithium ion adsorption column. The preparation method of the lithium slag based ion sieve adsorbent comprises the following steps: washing lepidolite smelting slag with water to remove impurities so as to obtain purified lithium slag; soaking the purified lithium slag in an acid solution, replacing lithium ions in the purified lithium slag, and separating the purified lithium slag from which the lithium ions are removed; placing the purified lithium slag without the lithium ions in a meta-aluminate solution, adjusting the pH value of the mixed solution to an acidic environment, and aging; and solid filter residues in the mixed solution are separated and dried, and the lithium slag-based ion sieve adsorbent is obtained. According to the lithium slag based ion sieve adsorbent disclosed by the invention, H2O.Al2O3. 4SiO2 is taken as a crystal nucleus, so that adsorption of Li < + > is promoted; the outer layer is coated with hydrophilic Al (OH) 3, so that the lithium slag-based ion sieve adsorbent has certain acid and alkali resistance, and Li < + > with smaller ion radius can penetrate through an Al (OH) 3 shell; the lithium slag-based ion sieve adsorbent has the advantages of high selectivity, good cyclic reproducibility and the like when being used for extracting lithium from salt lake brine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of resource utilization of lithium mica smelting slag, and in particular to a lithium slag-based ion sieve adsorbent and a preparation method thereof, and a lithium ion adsorption column. Background Art

[0002] Lithium is an important new energy metal, widely used in batteries, glass ceramics, aerospace and other fields. Salt lake brine is an important source of lithium resources, but due to its complex chemical composition, traditional lithium extraction technology has problems such as poor selectivity, low recycling rate and high cost. Summary of the invention

[0003] The present application provides a highly selective and reusable lithium slag-based ion sieve adsorbent and a preparation method thereof, and a lithium ion adsorption column.

[0004] In a first aspect, an embodiment of the present application provides a method for preparing a lithium slag-based ion sieve adsorbent, comprising the following steps:

[0005] Washing the lepidolite smelting slag with water to remove impurities to obtain purified lithium slag; wherein the lepidolite smelting slag comprises Li2O·Al2O3·4SiO2;

[0006] soaking the purified lithium slag in an acid solution to displace lithium ions in the purified lithium slag, and separating the purified lithium slag after the lithium ions are removed;

[0007] Placing the purified lithium slag after the lithium ions are removed in a metaaluminate solution, adjusting the pH of the mixed solution to an acidic environment and aging the mixed solution;

[0008] The solid filter residue in the mixed liquid is separated and dried to obtain a lithium slag-based ion sieve adsorbent.

[0009] According to the first aspect, in a possible implementation, the step of washing and removing impurities from the lithium mica smelting slag to obtain purified lithium slag comprises:

[0010] crushing the lepidolite smelting slag to obtain lepidolite smelting slag powder;

[0011] The lepidolite smelting slag powder is washed and settled to remove calcium, iron, magnesium, potassium and sodium oxides and sulfur trioxide.

[0012] According to the first aspect, in a possible implementation manner, the lithium mica smelting slag powder is sieved to 100 mesh to 200 mesh.

[0013] According to the first aspect, in a possible implementation, the step of soaking the purified lithium slag in an acid solution comprises:

[0014] The purified lithium slag is placed in a 0.1 mol / L to 0.5 mol / L hydrochloric acid solution and soaked for 60 min to 120 min.

[0015] According to the first aspect, in a possible implementation, the purified lithium slag after the removal of lithium ions is placed in a metaaluminate solution, and the pH of the mixed solution is adjusted to acidic, and the aging step includes:

[0016] placing the purified lithium slag after removal of lithium ions in a metaaluminate solution to obtain a mixed solution;

[0017] The pH of the mixed solution is adjusted to 3.0 to 5.0;

[0018] Aging for 30 to 60 minutes.

[0019] According to the first aspect, in a possible implementation manner, at least one of dilute hydrochloric acid, dilute sulfuric acid, and dilute nitric acid is added to the mixed solution to adjust the pH to 3.0-5.0.

[0020] According to the first aspect, in a possible implementation manner, the aluminate is at least one of sodium aluminate and potassium aluminate.

[0021] In a second aspect, an embodiment of the present application further provides a lithium slag-based ion sieve adsorbent, wherein the lithium slag-based ion sieve adsorbent is prepared by the preparation method of the lithium slag-based ion sieve adsorbent described in the first aspect.

[0022] In a third aspect, an embodiment of the present application further provides a lithium ion adsorption column, wherein the lithium ion adsorption column is filled with the lithium slag-based ion sieve adsorbent described in the second aspect.

[0023] According to the third aspect, in a possible implementation, solid phase microextraction gaskets are provided at both ends of the lithium slag-based ion sieve adsorbent along the axial direction of the lithium ion adsorption column.

[0024] The present application provides a lithium slag-based ion sieve adsorbent and a preparation method thereof, and a lithium ion adsorption column. The main component of the lithium slag-based ion sieve adsorbent is H2O·Al2O3·4SiO2, which is converted from a large amount of Li2O·Al2O3·4SiO2 in the lithium slag by acid washing. Under alkaline conditions, this reverse conversion will be beneficial to the reaction in the direction of lithium ion adsorption; at the same time, hydrophilic Al(OH)3 is coated on the outer layer of the lithium slag-based ion sieve adsorbent, so that the lithium slag-based ion sieve adsorbent has a certain acid and alkali resistance, and Li with a smaller ion radius can be adsorbed. + It can pass through the Al(OH)3 shell and act as a crystal nucleus inside the lithium slag lithium slag based ion sieve adsorbent to promote Li + Adsorption; lithium slag lithium slag based ion sieve adsorbent is used for lithium extraction from salt lake brine and has the advantages of high selectivity and good recycling regeneration. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] Figure 1 It is a schematic flow chart of a method for preparing a lithium slag-based ion sieve adsorbent in one embodiment of the present application;

[0027] Figure 2 is a schematic flow chart of a method for preparing a lithium slag-based ion sieve adsorbent in another embodiment of the present application;

[0028] Figure 3 1 is a schematic flow chart of a method for preparing a lithium slag-based ion sieve adsorbent in another embodiment of the present application;

[0029] Figure 4 is a schematic structural diagram of a lithium ion adsorption column in one embodiment of the present application;

[0030] Figure 5 is a scanning electron microscope image of a lithium slag-based ion sieve adsorbent in one embodiment of the present application;

[0031] Figure 6 This is a schematic diagram comparing the adsorption amount of lithium ions by lithium slag-based ion sieve adsorbent in lithium solutions with different pH values;

[0032] Figure 7 It is a schematic diagram comparing the selectivity of lithium slag-based ion sieve adsorbents for lithium ions;

[0033] Figure 8 It is a lithium ion adsorption column penetration curve diagram of lithium slag based ion sieve adsorbent;

[0034] Fig. 9 This is the adsorption-desorption cycle regeneration diagram of lithium ions by lithium slag-based ion sieve adsorbent.

[0035] Reference numerals:

[0036] 100. Lithium ion adsorption column; 11. Lithium slag-based ion sieve adsorbent; 12. Solid phase microextraction gasket. DETAILED DESCRIPTION

[0037] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0040] In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0041] Lithium has excellent physical and chemical properties such as high energy density, good conductivity and light weight. Therefore, it is widely used in lithium batteries, nuclear industry, aerospace and other fields, and is known as the "green energy metal". In recent years, with the expansion of the market for electric vehicles, 3C electronic products and energy storage equipment, the supply and demand of lithium resources have become increasingly tight, prompting scholars from various countries to explore various new technologies for extracting lithium from ores, seawater and salt lake brine. At present, about 60% to 70% of the world's proven lithium resources exist in the form of salt lake brine, and have great potential and long-term stability. However, due to the high sodium, potassium, magnesium and calcium content in salt lake brine and the low lithium content, it is very difficult to selectively extract lithium ions from salt lake brine. Therefore, the present application provides a highly selective and reusable lithium slag-based ion sieve adsorbent and its preparation method, and a lithium ion adsorption column.

[0042] In a first aspect, the present application provides a method for preparing a lithium slag-based ion sieve adsorbent, such as Figure 1 As shown, the following steps are included:

[0043] Step S10, washing and removing impurities from the lepidolite smelting slag to obtain purified lithium slag; wherein the lepidolite smelting slag comprises Li2O·Al2O3·4SiO2;

[0044] Li2O·Al2O3·4SiO2 in lepidolite smelting slag is its effective component.

[0045] In the process of lithium resource extraction and utilization, lithium mica smelting slag, as a by-product, often contains a large amount of underutilized lithium elements and other impurities such as calcium, iron, magnesium, potassium, sodium oxides and sulfur trioxide. Through the steps of water washing and impurity removal, the purity of lithium mica smelting slag can be effectively improved, and the above impurities can be avoided from remaining in the subsequent reaction to form undesirable by-products or reduce the extraction efficiency of lithium ions, laying the foundation for the efficient extraction of lithium ions in the subsequent steps.

[0046] Using lithium mica smelting slag as raw material not only reduces production costs, but also provides a new way for the bulk disposal of lithium mica smelting slag and its high-value utilization. It is of great significance to environmental protection and resource recycling, and has considerable economic and environmental benefits.

[0047] Specifically, Figure 2 As shown, step S10 includes:

[0048] Step S11, crushing the lepidolite smelting slag to obtain lepidolite smelting slag powder;

[0049] The lithium mica smelting slag is physically crushed by using equipment such as a crusher or a ball mill until it forms a powder.

[0050] By crushing, the particle size of the lithium mica smelting slag is reduced, and the surface area is significantly increased, thereby increasing the contact area between impurities and water in the subsequent water washing process, which is beneficial to the dissolution and removal of impurities.

[0051] In order to further improve the uniformity of the lithium mica smelting slag powder and the efficiency of subsequent treatment, the crushed lithium mica smelting slag powder can be screened using a screen, and the screen aperture is preferably 100 mesh to 200 mesh. Through screening, oversized or undersized particles can be removed, and the fineness and uniformity of the powder particles can be improved. Uniform particle size and fineness can improve the efficiency and consistency of chemical reactions, which is conducive to the full implementation of subsequent reactions.

[0052] Step S12, washing and settling the lepidolite smelting slag powder, and removing calcium, iron, magnesium, potassium and sodium oxides and sulfur trioxide.

[0053] The screened lithium mica smelting slag powder is placed in a cleaning device, and an appropriate amount of clean water is added for stirring and standing. Through water washing, soluble impurities such as oxides of calcium, iron, magnesium, potassium, sodium and sulfur trioxide are dissolved in water and separated from the lithium mica smelting slag powder by sedimentation.

[0054] According to the content and type of impurities, the number and intensity of water washing can be flexibly adjusted to ensure that the impurities are fully removed. If necessary, multi-stage water washing or countercurrent washing can be used to improve the impurity removal effect.

[0055] Step S20, soaking the purified lithium slag in an acid solution to displace lithium ions in the purified lithium slag, and separating the purified lithium slag after the lithium ions are removed;

[0056] The purified lithium slag is immersed in an acid solution to undergo the following reaction: Li2O·Al2O3·4SiO2+2H + →H2O·Al2O3·4SiO2+2Li + That is, a large amount of Li2O·Al2O3·4SiO2 in the purified lithium slag is converted into H2O·Al2O3·4SiO2 after acid washing. H2O·Al2O3·4SiO2, as the main component of the lithium slag-based ion sieve adsorbent, can be reversely converted under alkaline conditions to facilitate the reaction in the direction of lithium ion adsorption.

[0057] Based on the consideration of the solubility of lithium in lithium mica smelting slag, dilute hydrochloric acid with a concentration range of 0.1 mol / L to 0.5 mol / L can be selected, which can not only ensure the effective replacement of lithium ions, but also avoid the waste and safety hazards caused by excessive concentration.

[0058] In order to ensure that lithium ions can be fully replaced, the immersion time needs to be controlled. Generally speaking, the immersion time is set between 60 minutes and 120 minutes. The selection of this time range is based on the kinetic process of lithium ions dissolving from lithium slag into acid solution, which can not only ensure the effective leaching of lithium ions, but also avoid equipment corrosion and solution contamination that may be caused by immersion for too long.

[0059] In addition to controlling the soaking time, increasing stirring can significantly improve the contact efficiency between lithium slag and acid solution and accelerate the dissolution rate of lithium ions. At the same time, appropriately increasing the soaking temperature (but be careful not to exceed the temperature limit of the equipment) can also enhance the leaching effect. After the soaking is completed, the acid solution containing lithium ions is separated from the purified lithium slag after the lithium ions are removed by filtration or centrifugation. The purified lithium slag after the lithium ions are removed is used for further processing to form a lithium slag-based ion sieve adsorbent, and the acid solution of lithium ions can be used for lithium extraction and purification to make full use of the lithium in the lithium slag.

[0060] The specific concentration of the acid solution should be adjusted according to the mineralogical characteristics of the lithium slag, the lithium content and the target recovery rate to maximize the lithium leaching rate while reducing acid consumption.

[0061] Step S30, placing the purified lithium slag after removing lithium ions in a metaaluminate solution, adjusting the pH of the mixed solution to an acidic environment and aging;

[0062] The purified lithium slag after removal of lithium ions is placed in aluminate solution to undergo the following reaction: AlO2 - +H + +H2O→Al(OH)3↓, using H2O·Al2O3·4SiO2 as the nucleus to promote the adsorption of Li+, a hydrophilic Al(OH)3 coating layer is formed on the surface of H2O·Al2O3·4SiO2; the lithium slag-based ion sieve adsorbent has a certain acid and alkali resistance while maintaining the selective adsorption capacity for lithium ions; the pore size characteristics of the Al(OH)3 shell are used to allow Li+ with a smaller ion radius to be adsorbed. + Through the shell.

[0063] like Figure 3 As shown, step 30 includes:

[0064] Step S31, placing the purified lithium slag after removing lithium ions in a metaaluminate solution to obtain a mixed solution;

[0065] The purified lithium slag after removal of lithium ions is added to the aluminate solution, and stirred sufficiently to ensure that the lithium slag particles are evenly dispersed in the solution to form a mixed solution.

[0066] The aluminate may be selected from at least one of sodium aluminate and potassium aluminate, and the specific selection may be based on actual cost and effect.

[0067] Step S32, adjusting the pH of the mixed solution to 3.0-5.0;

[0068] At least one of dilute hydrochloric acid, dilute sulfuric acid, and dilute nitric acid is added to the mixed solution, and the pH value of the mixed solution is gradually adjusted to the range of 3.0 to 5.0 to trigger the reaction between AlO2- ions and H+ ions to generate Al(OH)3 precipitates.

[0069] It should be noted that the pH value should be adjusted slowly to avoid local over-acidification that may lead to structural destruction of the lithium slag or the generation of unnecessary by-products.

[0070] Step S33, aging for 30 to 60 minutes.

[0071] The mixed solution with adjusted pH value is placed in a static state for aging treatment. The aging time is generally controlled between 30 minutes and 60 minutes to ensure that Al(OH)3 can be fully precipitated and coated on the surface of lithium slag particles.

[0072] During the aging process, Al(OH)3 generated by the reaction of AlO2- ions and H+ ions will gradually deposit on the lithium slag particles to form a dense coating layer. This coating layer can not only improve the acid and alkali resistance of the lithium slag-based ion sieve adsorbent, but also achieve selective adsorption of Li+ through its pore size characteristics.

[0073] Step S40, separating the solid filter residue in the mixed solution and drying it to obtain a lithium slag-based ion sieve adsorbent.

[0074] After completing the aging process in the aluminate solution, the solid filter residue in the mixed solution (i.e., lithium slag-based ion sieve adsorbent coated with Al(OH)3) needs to be separated from the remaining liquid and dried to remove moisture, ultimately obtaining a dry and stable lithium slag-based ion sieve adsorbent.

[0075] Use appropriate solid-liquid separation equipment (such as filters, centrifuges, etc.) to separate the solid residue from the remaining liquid in the mixed liquid. The key to this step is to ensure that the solid residue can be completely separated from the mixed liquid while minimizing the loss of the residue.

[0076] The solid filter residue obtained by separation (i.e., lithium residue-based ion sieve adsorbent) is placed in a drying device, and the drying temperature is set to 70-80° C. This temperature range can effectively remove moisture without causing damage to the adsorbent structure or reduction in performance.

[0077] The drying time is usually 24 hours to ensure that the moisture in the adsorbent is completely removed. During the drying process, it is necessary to check the drying effect regularly to avoid insufficient drying or over-drying.

[0078] The lithium slag-based ion sieve adsorbent prepared by the present invention mainly comprises H2O·Al2O3·4SiO2 which is converted from a large amount of Li2O·Al2O3·4SiO2 in the lithium slag by acid washing. Under alkaline conditions, this reverse conversion is conducive to the reaction in the direction of lithium ion adsorption. At the same time, hydrophilic Al(OH)3 is coated on the outer layer of the lithium slag-based ion sieve adsorbent, so that the lithium slag-based ion sieve adsorbent has a certain acid and alkali resistance. Li+ with a smaller ion radius can pass through the Al(OH)3 shell and serve as a crystal nucleus inside the lithium slag-based ion sieve adsorbent to promote the adsorption of Li+. The lithium slag-based ion sieve adsorbent is used for lithium extraction from salt lake brine, and has the advantages of high selectivity and good recycling regeneration.

[0079] In the second aspect, the embodiment of the present application also provides a lithium slag-based ion sieve adsorbent, which is prepared by the preparation method of the lithium slag-based ion sieve adsorbent described in the first aspect. Therefore, the lithium slag-based ion sieve adsorbent is formed by a specific preparation process in the present application. Thanks to its unique surface structure and chemical properties, it can show extremely high selectivity for lithium ions (Li+) in a complex ion environment. This mainly enables lithium ions to be preferentially adsorbed on the surface or inside of the adsorbent, thereby effectively improving the extraction efficiency of lithium ions. And during the circulation of salt lake brine, the lithium slag-based ion sieve adsorbent can quickly respond and adsorb lithium ions in the solution. This feature makes the adsorption process more efficient and fast, which is conducive to the rapid extraction and enrichment of lithium resources. After adsorbing lithium ions, the lithium slag-based ion sieve adsorbent can release lithium ions through a simple dilute acid desorption process to obtain a lithium solution with higher purity; the lithium extraction process is simplified, and the purity of lithium products is improved, providing high-quality raw materials for subsequent processing and application. The regeneration of the lithium slag-based ion sieve adsorbent is also achieved. This cyclic regeneration capability not only reduces production costs, but also improves resource utilization efficiency. After multiple cycles of use, the performance of the lithium slag-based ion sieve adsorbent can still remain relatively stable, meeting the needs of long-term use.

[0080] Thirdly, Figure 4 As shown, the embodiment of the present application further provides a lithium ion adsorption column 100, in which the lithium ion adsorption column 100 is filled with the lithium slag-based ion sieve adsorbent 11 described in the second aspect. The lithium ion adsorption column 100 is filled with the lithium slag-based ion sieve adsorbent 11 with high selectivity and good recyclability described in the second aspect, which optimizes the adsorption and desorption process of lithium ions and improves the extraction efficiency of lithium resources.

[0081] The lithium ion adsorption column 100 can use a 6mL solid phase lithium ion adsorption column empty column tube to ensure sufficient space to accommodate the lithium slag-based ion sieve adsorbent 11 and allow the fluid to pass smoothly. 2 to 3g of the lithium slag-based ion sieve adsorbent 11 can be weighed to fill the lithium ion adsorption column 100, and the filling volume of the lithium slag-based ion sieve adsorbent 11 is 2 to 3mL. While ensuring sufficient adsorption capacity, avoid excessive resistance when the fluid passes.

[0082] Solid phase microextraction (SPME) gaskets 12 are provided at both ends of the lithium slag-based ion sieve adsorbent 11 along the axial direction of the lithium ion adsorption column 100. These SPME gaskets play the role of fixing the position of the lithium slag-based ion sieve adsorbent 11, preventing the lithium slag-based ion sieve adsorbent 11 from moving with the fluid, and improving the sealing performance. At the same time, the SPME gasket may also have selective adsorption capacity for specific compounds, further enhancing the performance of the lithium ion adsorption column 100.

[0083] Salt lake brine is pumped into the lithium ion adsorption column 100 at a constant speed by a flow pump. When the lithium ions in the brine flow through the lithium slag-based ion sieve adsorbent 11, they are efficiently adsorbed and fixed inside the lithium slag-based ion sieve adsorbent 11. This process achieves rapid enrichment and extraction of lithium ions. When the lithium ion adsorption column reaches saturation or lithium ions need to be recovered, a dilute acid solution can be pumped into the lithium ion adsorption column 100 by a flow pump. The dilute acid solution reacts with the lithium ions on the lithium slag-based ion sieve adsorbent 11, desorbs them from the lithium slag-based ion sieve adsorbent 11 and flows out with the solution. The desorbed lithium ions can be further processed to obtain a lithium solution with a higher purity.

[0084] In the first embodiment, 20g of lithium mica smelting slag is weighed for ball milling / vertical milling, and then passed through a 200 mesh sieve. The sieved lithium mica smelting slag is placed in a 250mL beaker and 100mL of water is added. It is stirred in an 80°C oil bath for 60min, filtered, repeated 2 to 3 times, and dried to obtain purified lithium mica smelting slag. The purified lithium mica smelting slag is placed in a 0.1mol / L hydrochloric acid solution for 120min to replace the lithium ions in the lithium mica smelting slag. 60g of sodium aluminate is weighed and dissolved in 100mL of water, ultrasonicated for 60min, and then mixed with the purified lithium mica smelting slag, the pH is adjusted to 4.0, the filter residue is filtered, and dried at 80°C for 24h to obtain Al(OH)3-coated lithium slag lithium slag-based ion sieve adsorbent.

[0085] The lepidolite smelting slag before and after purification was subjected to X-ray fluorescence spectrometer (XRF) test, as shown in Table 1. Table 1 is a table of chemical composition of the lepidolite smelting slag before and after impurity removal:

[0086] Table 1 Chemical composition of lithium mica smelting slag before and after impurity removal

[0087]

[0088] “-” means the content of the component is less than 0.0001

[0089] Comparing the composition of lithium mica smelting slag before and after water washing and impurity removal, the contents of iron oxide, magnesium oxide, sodium oxide, potassium oxide and sulfur trioxide in the lithium mica smelting slag decreased significantly after water washing, which shows that the impurity removal process effectively purified the lithium mica smelting slag.

[0090] See also Figure 5 , Figure 5 This is a scanning electron microscope (SEM) image of the lithium slag-based ion sieve adsorbent. Figure 5 It is shown in the figure that the surface of the lithium slag-based ion sieve adsorbent is covered with dense Al(OH)3 spherical particles, which plays a protective role on the lithium slag-based ion sieve adsorbent made from lithium mica smelting slag.

[0091] In the second embodiment, based on the lithium slag-based ion sieve adsorbent prepared in the first embodiment, 2.87 g of lithium slag-based ion sieve adsorbent material was weighed and filled into a lithium ion adsorption column, and the filling volume of the lithium slag-based ion sieve adsorbent was 2 mL (1BV=2 mL); the lithium ion adsorption column used a 6 mL solid phase lithium ion adsorption column empty column tube, and the top and bottom of the filling material were sealed with SPME gaskets.

[0092] The simulated salt lake brine composition is 0.0989g / L Li + , 0.3629g / LK + 、96.54g / LNa + , 1.718 g / L Ca 2+ 、0.8619g / LMg 2+ The volume of simulated salt lake brine introduced was 200 mL; the flow pump pumped at a constant speed of 0.5 mL / min.

[0093] 100 mL of 0.5 mol / L dilute hydrochloric acid solution was pumped into the lithium ion adsorption column filled with lithium slag-based ion sieve adsorbent at a speed of 0.5 mL / min through a flow pump, thereby completing the desorption of lithium ions from the lithium slag-based ion sieve adsorbent to obtain an enriched LiCl solution.

[0094] In the third embodiment, 20 mL of lithium chloride aqueous solution with a lithium element of 300 mg / L at pH values ​​of 2, 3, 4, 5, 6, 7, 8, 9, 10, and 11 are respectively prepared; 20 mL of lithium ion solutions with different pH values ​​are respectively placed in 10 50 mL conical flasks; the reagents for adjusting the acidity and alkalinity of the lithium ion solution are 0.1 mol / L hydrochloric acid solution and 0.1 mol / L sodium hydroxide solution;

[0095] Weigh 20 mg of the lithium slag-based ion sieve adsorbent prepared in the first embodiment, a total of 10 parts, and put the weighed materials into conical flasks containing aqueous solutions with a lithium concentration of 300 mg / L at pH 2, 3, 4, 5, 6, 7, 8, 9, 10, and 11, respectively, and put them into a constant temperature oscillator with parameters set to 25°C, 180 rpm, and 24h for adsorption experiment;

[0096] The ion solutions before and after adsorption in the conical flask were taken and filtered through a 0.22 μm filter screen, and the lithium ion concentration in the solution was determined using an atomic absorption spectrometer (AAS).

[0097] The adsorption behavior of the prepared lithium slag-based ion sieve adsorbent under different pH conditions was tested. Figure 6A schematic diagram comparing the adsorption amount of lithium ions by lithium slag-based ion sieve adsorbent in lithium solutions with different pH values, specifically a diagram showing the change in the adsorption amount of lithium ions by the lithium slag-based ion sieve adsorbent in lithium solutions with a pH value of 2-11, used to illustrate the effect of pH on the adsorption of lithium ions; in acidic solutions with a pH value of 2-5, the adsorption amount of lithium ions by the lithium slag-based ion sieve adsorbent is maintained at approximately 8.5 mg / g, indicating that the acidic solution has little effect on the adsorption amount of the lithium slag-based ion sieve adsorbent; in alkaline solutions with a pH value of 7-11, the adsorption amount of lithium ions by the lithium slag-based ion sieve adsorbent shows an upward trend, with a maximum adsorption amount of 16.48 mg / g, indicating that alkaline conditions promote the adsorption of lithium ions by the lithium slag-based ion sieve adsorbent.

[0098] In the fourth embodiment, a mixed solution of 2mmol / L lithium ions, 2mmol / L potassium ions, 2mmol / L sodium ions, 2mmol / L calcium ions and 2mmol / L magnesium ions is prepared, and the volume is 20mL; the mixed solution is placed in a 50mL conical flask; the reagents used to prepare the mixed solution are lithium chloride, potassium chloride, sodium chloride, calcium chloride and magnesium chloride respectively;

[0099] Weigh 20 mg of the lithium slag-based ion sieve adsorbent prepared in the first embodiment, a total of 2 portions, respectively put into a mixed solution containing 2 mmol / L of lithium ions, 2 mmol / L of potassium ions, 2 mmol / L of sodium ions, 2 mmol / L of calcium ions and 2 mmol / L of magnesium ions, and put it into a constant temperature oscillator with parameters set to 25°C, 180 rpm, and 24 h for adsorption experiment;

[0100] The ion solutions before and after adsorption in the conical flask were taken and passed through a 0.22 μm filter screen, and the concentrations of lithium ions, potassium ions, sodium ions, calcium ions and magnesium ions in the solution were determined using inductively coupled plasma mass spectrometry (ICP MS).

[0101] The selective adsorption capacity of the prepared lithium slag-based ion sieve adsorbent for lithium ions was measured:

[0102] Figure 7 This is a schematic diagram of the selectivity comparison of the lithium slag-based ion sieve adsorbent for lithium ions, showing the adsorption of the lithium slag-based ion sieve adsorbent in a mixed solution of lithium, potassium, sodium, calcium and magnesium. Figure 7 It is shown that the adsorption capacity of potassium ions, sodium ions, calcium ions and magnesium ions by the lithium slag-based ion sieve adsorbent is not high (<0.34mmol / g). In contrast, the adsorption effect on lithium ions is significant (1.51mmol / g), indicating that the lithium slag-based ion sieve adsorbent is selective for the adsorption of lithium ions.

[0103] In the fifth embodiment, 2.87 g of the lithium slag-based ion sieve adsorbent is weighed and filled into a lithium ion adsorption column, and the filling volume of the lithium slag-based ion sieve adsorbent is 2 mL (1BV=2 mL); the lithium ion adsorption column uses a 6 mL solid phase lithium ion adsorption column empty column tube, and the top and bottom of the filling material are sealed with SPME gaskets;

[0104] The simulated salt lake brine was pumped into the lithium ion adsorption column at a constant speed of 0.5 mL / min by a flow pump. The volume of the simulated brine introduced was 200 mL. The composition of the simulated salt lake brine was 0.0989 g / L Li + , 0.3629g / LK + 、96.54g / LNa + 、1.718g / LCa 2+ 、0.8619g / LMg 2+ ;

[0105] The simulated salt lake brine treated with lithium slag-based ion sieve adsorbent was sampled every 5 mV, passed through a 0.22 μm filter, and the lithium ion concentration in the solution was determined using an atomic absorption spectrometer (AAS).

[0106] The adsorption capacity of the prepared lithium slag-based ion sieve adsorbent for salt lake brine was measured as follows: Figure 8 This is a lithium ion adsorption column penetration curve of the lithium slag-based ion sieve adsorbent, which tests the ability of the lithium slag-based ion sieve adsorbent to dynamically adsorb lithium ions. Figure 8 It is shown that the lithium ions in the 0-80 mV simulated salt lake brine solution treated with lithium slag-based ion sieve adsorbent are well adsorbed (C e / C0<0.02), the adsorption effect of lithium slag based ion sieve adsorbent on lithium ions in 80-130mV simulated salt lake brine solution gradually decreased, and the adsorption effect of lithium slag based ion sieve adsorbent on lithium ions was basically invalid in 130-200mV simulated salt lake brine solution, indicating that the lithium slag based ion sieve adsorbent has a good ability to dynamically adsorb lithium ions and has the potential for industrial application.

[0107] In the sixth embodiment, a lithium chloride aqueous solution with a lithium element concentration of 100 mg / L is prepared, and 50 mL of the solution with this concentration is taken into a 100 mL conical flask; a hydrochloric acid solution with a concentration of 0.5 mol / L is prepared as a desorption solution;

[0108] Weigh 50 mg of the prepared lithium slag-based ion sieve adsorbent, put it into an aqueous solution containing 100 mg / L of lithium ions, and put it into a constant temperature oscillator with parameters set at 25°C, 180 rpm, and 12 h for adsorption experiment;

[0109] The ion solution before and after adsorption in the conical flask was taken, and the lithium ion concentration in the solution was determined using an atomic absorption spectrometer (AAS);

[0110] 50 mg of the lithium slag-based ion sieve adsorbent in (2) was separated by suction filtration, put into 50 mL of 0.5 mol / L hydrochloric acid solution, and placed in a constant temperature oscillator with parameters set at 25°C, 180 rpm, and 12 h for desorption experiment;

[0111] The ion solutions before and after desorption in the conical flask were taken, and the lithium ion concentration in the solution was determined using an atomic absorption spectrometer (AAS); the above steps were repeated five times.

[0112] The adsorption-desorption cycle regeneration capacity of the prepared lithium slag-based ion sieve adsorbent was measured as follows: Fig. 9 The adsorption-desorption cycle regeneration diagram of lithium ions by the lithium slag-based ion sieve adsorbent shows that the lithium slag-based ion sieve adsorbent can be recycled for more than 5 times. The adsorbent has good regeneration ability and can be recycled.

[0113] In the seventh embodiment, a 0.5 mol / L hydrochloric acid solution is pumped into the lithium ion adsorption column treated with the simulated salt lake brine by a flow pump at a constant speed of 0.5 mL / min, and the volume of the hydrochloric acid solution introduced is 100 mL;

[0114] The desorbed hydrochloric acid solution and the original simulated salt lake brine were taken separately, passed through a 0.22 μm filter screen, and the concentrations of lithium ions, potassium ions, sodium ions, calcium ions and magnesium ions in the solution were determined using inductively coupled plasma mass spectrometry (ICP MS).

[0115] The desorption of lithium ions from the lithium slag-based ion sieve adsorbent was measured:

[0116] Table 2 Concentrations of metal cations in simulated salt lake brine and desorption solution

[0117] Solution / (g / L) <![CDATA[Li + ]]> <![CDATA[K + ]]> <![CDATA[Na + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> Simulated brine 0.0989 0.3629 96.54 1.718 0.8619 Desorption liquid 0.0887 0.0017 0.0179 0.0141 0.0107

[0118] Table 2 is a comparison of the concentration of various cations in the desorption liquid and the original simulated salt lake brine after the lithium slag-based ion sieve adsorbent that adsorbed lithium ions is desorbed. The data in the table show that the concentrations of cations such as potassium, sodium, calcium, and magnesium in the original simulated brine are much greater than the concentration of lithium ions; the lithium ion adsorption column filled with the lithium slag-based ion sieve adsorbent is treated, and then the desorption liquid is used to desorb lithium ions; the desorption liquid is mainly lithium ions, containing a small amount of potassium, sodium, calcium, and magnesium ions; This shows that the present invention can effectively and selectively extract lithium resources from salt lake brine.

[0119] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

[0120] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a lithium slag-based ion sieve adsorbent, It is characterized in that The following steps are involved: The lithium mica smelting slag is washed with water to remove impurities to obtain purified lithium slag; wherein the lithium mica smelting slag includes Li 2 O.Al 2 O 3 ·4SiO 2 ; soaking the purified lithium slag in an acid solution to displace lithium ions in the purified lithium slag, and separating the purified lithium slag after the lithium ions are removed; Placing the purified lithium slag after the lithium ions are removed in a metaaluminate solution, adjusting the pH of the mixed solution to an acidic environment and aging the mixed solution; The solid filter residue in the mixed liquid is separated and dried to obtain a lithium slag-based ion sieve adsorbent.

2. The method for preparing the lithium slag-based ion sieve adsorbent according to claim 1, It is characterized in that The step of washing and removing impurities from the lepidolite smelting slag to obtain purified lithium slag comprises: crushing the lepidolite smelting slag to obtain lepidolite smelting slag powder; The lepidolite smelting slag powder is washed and settled to remove calcium, iron, magnesium, potassium and sodium oxides and sulfur trioxide.

3. The method for preparing the lithium slag-based ion sieve adsorbent according to claim 2, It is characterized in that The lithium mica smelting slag powder is sieved to 100 mesh to 200 mesh.

4. The method for preparing the lithium slag-based ion sieve adsorbent according to claim 1, It is characterized in that The step of soaking the purified lithium slag in an acid solution comprises: The purified lithium slag is placed in a 0.1 mol / L to 0.5 mol / L hydrochloric acid solution and soaked for 60 min to 120 min.

5. The method for preparing the lithium slag-based ion sieve adsorbent according to claim 1, It is characterized in that The step of placing the purified lithium slag after removing lithium ions in a metaaluminate solution and adjusting the pH of the mixed solution to acidic, and aging comprises: placing the purified lithium slag after removal of lithium ions in a metaaluminate solution to obtain a mixed solution; The pH of the mixed solution is adjusted to 3.0-5.0; Aging for 30 to 60 minutes.

6. The method for preparing the lithium slag-based ion sieve adsorbent according to claim 5, It is characterized in that At least one of dilute hydrochloric acid, dilute sulfuric acid and dilute nitric acid is added to the mixed solution to adjust the pH to 3.0-5.

0.

7. The method for preparing the lithium slag-based ion sieve adsorbent according to claim 1, It is characterized in that The aluminate is at least one of sodium aluminate and potassium aluminate.

8. A lithium slag-based ion screen adsorbent, It is characterized in that The lithium slag-based ion sieve adsorbent is prepared by the preparation method of the lithium slag-based ion sieve adsorbent according to any one of claims 1 to 8.

9. A lithium ion adsorption column, It is characterized in that The lithium ion adsorption column is filled with the lithium slag-based ion sieve adsorbent as claimed in claim 8.

10. The lithium ion adsorption column according to claim 9, It is characterized in that Along the axial direction of the lithium ion adsorption column, solid phase microextraction gaskets are arranged at both ends of the lithium slag-based ion sieve adsorbent.

Citation Information

Patent Citations

  • Preparation method of lithium slag adsorbent for liquid extraction of lithium

    CN103706325A

  • Aluminum-based lithium ion sieve as well as preparation method and application thereof

    CN112808226A

  • Method for preparing lithium ion sieve by using nepheline

    CN116282061A

Cited By

  • Method for regulating and controlling viscosity of mineral wool melt from spodumene lithium extraction tailings