Composite material capable of synchronously adsorbing radioactive iodide ions and cesium ions and preparation method thereof
Through the preparation of Elosite-based composite materials, the hydrothermal carbon film and silver oxide nanoparticles are used to solve the problem of difficulty in adsorbing radioactive iodine and cesium ions simultaneously in the prior art, achieving efficient synchronous adsorption effect and reducing Preparation of energy consumption and pollution.
Patent Information
- Application Number
- CN202411008346.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
Existing adsorbent materials are difficult to efficiently adsorb radioactive iodine ions (I-) and cesium ions (Cs+) present in the environment at the same time, which often exists at the same time in the environment, resulting in poor adsorption effect.
Using Elosite-based composite material, through electric heat drying, ultrasonic dispersion, hydrothermal reaction, addition of glucose and acrylic acid and silver nitrate solution treatment, a composite material covering hydrothermal carbon film and silver oxide nanoparticles is formed to achieve I- and Synchronous adsorption of Cs+.
This material can stably and synchronize the adsorption of iodine and cesium ions, with adsorption amounts reaching 1.05mmol/g and 0.63mmol/g respectively. When the initial concentration of cesium iodide solution is 2mmol/L, the adsorption capacity of the two ions is significantly improved. , and the preparation process is low temperature and low energy consumption, and natural nanotube minerals are used to avoid strong contamination of chemical reagents.
Smart Images

Figure CN118925664A_ABST
Abstract
Description
Technical field:
[0001] The invention belongs to the technical field of mineral materials, and in particular relates to a halloysite-based composite material capable of synchronously adsorbing radioactive iodine ions and cesium ions and a preparation method thereof. Background technology:
[0002] Nuclear energy has been widely used in fields such as nuclear power and military. The development of the nuclear industry inevitably produces a large amount of spent fuel and nuclear waste, posing a severe challenge to the living environment of mankind. Iodine and cesium are two important radioactive nuclides. Due to their high radiotoxicity and solubility, as well as their strong migration ability in the environment, their effective adsorption continues to attract research attention (Gao Can et al., Environmental Chemistry, 2014; Su Minhua et al., Water Treatment Technology, 2023). - and Cs + They are anionic and cationic pollutants respectively. The adsorbents currently used are often - or Cs + It is difficult to achieve the simultaneous adsorption of two ions. For example, montmorillonite has a high cation exchange capacity for Cs + It has a high adsorption capacity (Long H., et al., Chem. Eng. J., 2013). - It does not have adsorption capacity (Miller A., et al., J. Environ. Radioact., 2015). In the actual environment, I - and Cs + Often exist at the same time (Kim J., et al., J. Environ. Chem. Eng., 2022), therefore, new adsorption materials need to be developed to achieve I - and Cs + Synchronous adsorption. Summary of the invention:
[0003] The purpose of the present invention is to treat the coexistence of radioactive iodine and cesium in the environment, where iodine is in the form of anions (I - ) and cesium in the form of cations (Cs + ) exists, and the adsorption material in the prior art only has an adsorption effect on one of the ions. The present invention provides a halloysite-based composite material and a preparation method thereof, and the composite material can achieve the simultaneous adsorption of iodide ions and cesium ions.
[0004] The technical solution of the present invention is: a method for preparing a composite material for synchronously adsorbing radioactive iodine ions and cesium ions, comprising the following steps:
[0005] S1. Dry the halloysite in an electric blast drying oven at 120° C. for 12 to 24 hours, mix the dried halloysite with ultrapure water, disperse it by ultrasonication, and stir it evenly on a magnetic stirrer to obtain a halloysite suspension;
[0006] S2, adding glucose to the halloysite suspension and stirring evenly to form a halloysite glucose suspension;
[0007] S3, adding acrylic acid to the halloysite-glucose suspension and stirring evenly to obtain a halloysite-organic suspension, and transferring the halloysite-organic suspension to the lining of a hydrothermal reactor for hydrothermal reaction;
[0008] S4, naturally cooling the suspension obtained by the hydrothermal reaction, separating the solid and the liquid, washing, and drying the solid phase at 80° C. to obtain a halloysite hydrothermal carbon composite material;
[0009] S5. The halloysite hydrothermal carbon composite material and the silver nitrate solution are mixed in proportion to obtain a suspension, the suspension is placed in a conical flask, an alkali solution is added dropwise into the conical flask at a rate of 0.1 mL / min, and the mixture is stirred at room temperature for 2-8 h. After the reaction is completed, the solid-liquid separation and washing are performed, and the solid phase is dried at 80° C. to obtain a halloysite-based composite material that simultaneously adsorbs radioactive iodine ions and cesium ions.
[0010] Furthermore, the purity of the halloysite is greater than 70wt%.
[0011] Furthermore, the mixing ratio of the halloysite and the ultrapure water in step S1 is 1 g / 70 mL.
[0012] Furthermore, the amount of glucose used in step S2 is: 5 g glucose / 1 g halloysite.
[0013] Furthermore, the amount of acrylic acid used in step S3 is: 10-14 mL acrylic acid / 1 g halloysite.
[0014] Furthermore, the conditions of the hydrothermal reaction in step S3 are: hydrothermal temperature is 160° C., and reaction time is 12 h.
[0015] Furthermore, the washing in step S4 is specifically washing with ultrapure water and ethanol alternately.
[0016] Furthermore, the solid-liquid separation in step S4 and step S5 is performed by centrifugation or filtration.
[0017] Furthermore, the concentration of the silver nitrate solution in step S5 is 10-100 mmol / L.
[0018] Furthermore, the alkaline solution in step S5 is an aqueous solution of NaOH, KOH or LiOH with a concentration of 0.01-0.1 mol / L.
[0019] Furthermore, in step S5, the halloysite hydrothermal carbon composite material is mixed with the silver nitrate solution at a solid-liquid ratio of 1 g / 100 mL, and the amount of the alkaline solution added is a ratio of the mass of the halloysite hydrothermal carbon composite material to the volume of the alkaline solution of 1 g / 10 mL.
[0020] The halloysite-based composite material obtained by the preparation method has a structure in which a hydrothermal carbon film is coated on the surface of the halloysite, and silver oxide nanoparticles are precipitated on the surface of the carbon film.
[0021] The halloysite-based composite material is used for synchronously adsorbing radioactive iodine ions and cesium ions.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] 1. The carrier halloysite used in the present invention is a natural nano-tubular mineral, which has the advantages of stable structure, low cost and easy availability; and the present invention does not use highly polluting chemical reagents, except for the hydrothermal reaction, it is completed at a relatively low temperature (the hydrothermal temperature is also relatively low), and the reaction time is short, which is conducive to shortening the preparation cycle of the composite material and reducing production energy consumption.
[0024] 2. The alkaline solution used in the present invention not only provides an alkaline environment for the growth of Ag2O nanoparticles, so that the Ag2O nanoparticles are precipitated on the surface of the halloysite hydrothermal carbon composite material; but also can further activate the composite material, increase the number of active groups such as carboxyl and hydroxyl groups on the surface of the composite material, improve the reaction activity such as the charge of the composite material, and thus improve the adsorption capacity of the composite material for cesium.
[0025] 3. The halloysite-based composite material prepared by the method of the present invention has the advantages of stable structure and can simultaneously adsorb iodide ions and cesium ions. When the initial concentration of the cesium iodide solution is 2 mmol / L, the composite material has an adsorption capacity of iodide ions and cesium ions. - and Cs + The adsorption amounts can reach 1.05mmol / g and 0.63mmol / g respectively. Description of the drawings:
[0026] Figure 1 Figures (a) and (b) are transmission electron microscope images of the halloysite used in Example 1 and the composite material prepared therefrom. Figure (c) and (d) are TEM images and energy spectrum images of the halloysite-based composite material prepared in Example 1 for simultaneous adsorption of radioactive iodine ions and cesium ions, respectively.
[0027] Figure 2The synchronous adsorption diagrams of radioactive nuclide iodine ions and cesium ions by the halloysite-based composite materials and the halloysite hydrothermal carbon composite materials for synchronous adsorption of radioactive iodine ions and cesium ions prepared in Examples 1, 2 and Comparative Example 1 are shown. (a) is the adsorption diagram of radioactive iodine ions by each composite material; and (b) is the adsorption diagram of radioactive cesium ions by each composite material. Specific implementation method:
[0028] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0029] Example 1
[0030] The halloysite was placed in a vacuum drying oven and dried at 120°C for 12 hours under vacuum conditions; 1 g of the dried halloysite was mixed with 70 mL of ultrapure water, ultrasonicated for 30 minutes, and then placed in a magnetic stirrer and stirred for 30 minutes to obtain a halloysite suspension; 5 g of glucose was added to the halloysite suspension, and stirred for 30 minutes to obtain a halloysite glucose suspension; 10 mL of acrylic acid was added to the halloysite glucose suspension, stirred for 30 minutes, and then transferred to the lining of a hydrothermal reactor for hydrothermal reaction at 160°C for 12 hours; the suspension obtained by the hydrothermal reaction was naturally cooled and transferred to a centrifuge tube for solid-liquid separation and ultrapure water was used to purify the suspension. and ethanol alternately washed 6 times, the solid phase was dried at 80 ° C to obtain a halloysite hydrothermal carbon composite material; 0.5g of the dried halloysite hydrothermal carbon composite material was mixed with 50mL of 100mmol / L silver nitrate solution to obtain a suspension, which was placed in a conical flask, and a NaOH solution with a concentration of 0.01mol / L was added dropwise according to the mass / alkaline solution volume ratio of the halloysite hydrothermal carbon composite material to 1g / 10mL. The mixture was fully stirred at room temperature for 2h, centrifuged and washed after the reaction, and the solid phase was dried at 80 ° C to obtain a halloysite-based composite material that can simultaneously adsorb radioactive iodine ions and cesium ions. Figure 1 The following are transmission electron microscope images of the halloysite used in Example 1 and the composite material prepared therefrom. Figure (a) is a transmission electron microscope image of the halloysite used in the example; Figure (b) is a transmission electron microscope image of the halloysite hydrothermal carbon composite material prepared in Example 1; Figures (c) and (d) are TEM images and energy spectrum images of the halloysite-based composite material for synchronous adsorption of radioactive iodine ions and cesium ions prepared in Example 1, respectively. Through transmission electron microscope analysis, it was found that in the halloysite-based composite material for synchronous adsorption of radioactive iodine ions and cesium ions, hydrothermal carbon formed a uniform carbon film on the surface of the halloysite, and Ag2O nanoparticles were relatively uniformly distributed on the halloysite hydrothermal carbon film.
[0031] As an implementation application, an adsorption experiment was carried out at room temperature according to a solid-liquid ratio of 0.1 g of the halloysite-based composite material for adsorbing radioactive iodine ions and cesium ions / 100 mL of cesium iodide solution. When the initial concentration of the cesium iodide solution was 2 mmol / L, the halloysite-based composite material for adsorbing radioactive iodine ions and cesium ions had an adsorption capacity of 1. - and Cs + The adsorption amounts were 1.05mmol / g and 0.63mmol / g respectively.
[0032] Example 2
[0033] The halloysite was placed in a vacuum drying oven and dried at 120°C for 12 hours under vacuum conditions; 1 g of the dried halloysite was mixed with 70 mL of ultrapure water, ultrasonicated for 30 minutes, and then stirred in a magnetic stirrer for 30 minutes to obtain a halloysite suspension; 5 g of glucose was added to the halloysite suspension and stirred for 30 minutes to obtain a halloysite glucose suspension; 10 mL of acrylic acid was added to the halloysite glucose suspension, stirred for 30 minutes, and then transferred to the lining of a hydrothermal reactor for hydrothermal reaction at 160°C for 12 hours; the suspension obtained by the hydrothermal reaction was naturally cooled and transferred to a centrifuge tube for solid-liquid separation and ultrapure water was used to purify the suspension. and ethanol alternately washed 6 times, the solid phase was dried at 80 ° C to obtain a halloysite hydrothermal carbon composite material; 0.5g of the dried halloysite hydrothermal carbon composite material was mixed with 50mL of a 10mmol / L silver nitrate solution to obtain a suspension, which was placed in a conical flask, and a 0.01mol / L NaOH solution was added dropwise according to the mass / alkaline solution volume ratio of the halloysite hydrothermal carbon composite material to 1g / 10mL. The mixture was fully stirred at room temperature for 2h, centrifuged and washed after the reaction, and the solid phase was dried at 80 ° C to obtain a halloysite-based composite material that can simultaneously adsorb radioactive iodine ions and cesium ions.
[0034] As an implementation application, an adsorption experiment was carried out at room temperature according to a solid-liquid ratio of 0.1 g of the halloysite-based composite material for adsorbing radioactive iodine ions / 100 mL of cesium iodide solution. When the initial concentration of the cesium iodide solution was 2 mmol / L, the halloysite-based composite material for adsorbing radioactive iodine ions and cesium ions had an adsorption capacity of 1. - and Cs + The adsorption amounts were 0.82mmol / g and 0.61mmol / g respectively.
[0035] Example 3
[0036] The halloysite was placed in a vacuum drying oven and dried at 120°C for 24 hours under vacuum conditions; 1 g of the dried halloysite was mixed with 70 mL of ultrapure water, subjected to ultrasonication for 30 minutes, and then stirred in a magnetic stirrer for 30 minutes to obtain a halloysite suspension; 5 g of glucose was added to the halloysite suspension and stirred for 30 minutes to obtain a halloysite glucose suspension; 14 mL of acrylic acid was added to the halloysite glucose suspension and stirred for 30 minutes; the suspension was then transferred to the inner lining of a hydrothermal reactor and subjected to hydrothermal reaction at 160°C for 12 hours; the suspension obtained in the hydrothermal reactor was naturally cooled and then transferred to a centrifuge tube for solid-liquid separation and ultrapure The mixture was washed alternately with water and ethanol for 6 times, and the solid phase was dried at 80°C to obtain a halloysite hydrothermal carbon composite material; 0.5 g of the dried halloysite hydrothermal carbon composite material was mixed with 50 mL of a 10 mmol / L silver nitrate solution to obtain a suspension, which was placed in a conical flask, and a 0.1 mol / L NaOH solution was added dropwise according to a mass / alkaline solution ratio of 1 g / 10 mL of the halloysite hydrothermal carbon composite material. The mixture was stirred at room temperature for 8 hours. After the reaction was completed, the mixture was centrifuged and washed, and the solid phase was dried at 80°C to obtain a halloysite-based composite material that can simultaneously adsorb radioactive iodine ions and cesium ions.
[0037] As an implementation application, the adsorption experiment was carried out at room temperature according to the solid-liquid ratio of 0.1g of the halloysite-based composite material for adsorbing radioactive iodine ions / 100mL of cesium iodide solution. When the initial concentration of the cesium iodide solution was 2mmol / L, the halloysite-based composite material for adsorbing radioactive iodine ions and cesium ions had a significant effect on the adsorption of I- and Cs + The adsorption amounts were 0.79 mmol / g and 0.55 mmol / g respectively.
[0038] Comparative Example 1
[0039] The halloysite was placed in a vacuum drying oven and dried at 120°C for 12 hours under vacuum conditions; 1 g of the dried halloysite was mixed with 70 mL of ultrapure water, ultrasonicated for 30 minutes, and then placed in a magnetic stirrer and stirred for 30 minutes to obtain a halloysite suspension; 5 g of glucose was added to the halloysite suspension, and stirred for 30 minutes to obtain a halloysite glucose suspension; 10 mL of acrylic acid was added to the halloysite glucose suspension, stirred for 30 minutes, and then the suspension was transferred to the lining of a hydrothermal reactor and hydrothermally reacted at 160°C for 12 hours; the suspension in the naturally cooled reactor was transferred to a centrifuge tube, the solid-liquid separation was carried out, and the ultrapure water and ethanol were alternately washed for 6 times, and the solid phase was dried at 80°C to obtain a halloysite hydrothermal carbon composite material for comparison;
[0040] As a comparative example, an adsorption experiment was carried out at room temperature according to a solid-liquid ratio of 0.1 g of the comparative halloysite hydrothermal carbon composite material / 100 mL of cesium iodide solution. Figure 2The synchronous adsorption diagrams of radioactive iodine ions and cesium ions by the halloysite-based composite materials and the halloysite hydrothermal carbon composite materials prepared in Examples 1, 2 and Comparative Example 1. (a) is the adsorption diagram of radioactive iodine ions by each composite material; (b) is the adsorption diagram of radioactive iodine ions by each composite material. When the initial concentration of the cesium iodide solution is 2 mmol / L, the halloysite-based composite materials used for comparison have a high adsorption rate of I- and Cs + The adsorption amounts of Cs and s were 0.016mmol / g and 0.15mmol / g respectively. This result shows that the halloysite hydrothermal carbon composite material used for comparison only has a + It has a certain adsorption capacity for I - The adsorption amount is extremely low; comparing the adsorption results of Example 1 and Example 1, it can be seen that the technical step of growing Ag2O particles onto the halloysite hydrothermal carbon composite material of the present invention not only significantly improves the composite material on I - The adsorption capacity of the composite material to Cs + The adsorption capacity of I - and Cs + Synchronous and efficient adsorption.
[0041] Comparative Example 2: The halloysite is placed in a vacuum drying oven and dried at 120°C for 12 h under vacuum conditions; 0.5 g of the dried halloysite is mixed with 50 mL of a 100 mmol / L silver nitrate solution to obtain a suspension, which is placed in a conical flask, and a 0.01 mol / L NaOH solution is added dropwise according to a halloysite mass / alkaline solution volume ratio of 1 g / 10 mL. The mixture is fully stirred at room temperature for 2 h. After the reaction is completed, the mixture is centrifuged and washed, and the solid phase is dried at 80°C to obtain a halloysite Ag2O composite material for comparison.
[0042] As an implementation application, an adsorption experiment was carried out at room temperature according to a solid-liquid ratio of 0.1 g of the comparative halloysite Ag2O composite material / 100 mL of cesium iodide solution. When the initial concentration of the cesium iodide solution was 2 mmol / L, the comparative halloysite Ag2O composite material had an adsorption capacity of 1 - and Cs + The adsorption amounts of the halloysite Ag2O composite materials used for comparison were 0.16mmol / g and 0.13mmol / g, respectively. - and Cs + The adsorption capacity of the composite material is relatively low. By comparing the adsorption results of Example 2 and Example 1, it can be seen that the technical steps of the present invention firstly coat a hydrothermal carbon film on the surface of the halloysite and then precipitate Ag2O nanoparticles on the surface of the hydrothermal carbon film, and at the same time improve the adsorption of the composite material on I - and Cs + adsorption capacity.
Claims
1. A method for preparing a composite material for synchronously adsorbing radioactive iodine ions and cesium ions, characterized in that: The following steps are involved: S1. Dry the halloysite in an electric blast drying oven at 120° C. for 12 to 24 hours, mix the dried halloysite with ultrapure water, disperse it by ultrasonication, and stir it evenly on a magnetic stirrer to obtain a halloysite suspension; S2, adding glucose to the halloysite suspension and stirring evenly to form a halloysite glucose suspension; S3, adding acrylic acid to the halloysite-glucose suspension and stirring evenly to obtain a halloysite-organic suspension, and transferring the halloysite-organic suspension to the lining of a hydrothermal reactor for hydrothermal reaction; S4, naturally cooling the suspension obtained by the hydrothermal reaction, separating the solid and the liquid, washing, and drying the solid phase at 80° C. to obtain a halloysite hydrothermal carbon composite material; S5. The halloysite hydrothermal carbon composite material and the silver nitrate solution are mixed in proportion to obtain a suspension, the suspension is placed in a conical flask, an alkali solution is added dropwise into the conical flask at a rate of 0.1 mL / min, and the mixture is stirred at room temperature for 2-8 h. After the reaction is completed, the solid-liquid separation and washing are performed, and the solid phase is dried at 80° C. to obtain a halloysite-based composite material that simultaneously adsorbs radioactive iodine ions and cesium ions.
2. The preparation method according to claim 1, characterized in that: The mixing ratio of halloysite and ultrapure water in step S1 is 1 g / 70 mL.
3. The preparation method according to claim 1, characterized in that: The amount of glucose used in step S2 is: 5 g glucose / 1 g halloysite.
4. The preparation method according to claim 1, characterized in that: The amount of acrylic acid used in step S3 is: 10-14 mL acrylic acid / 1 g halloysite.
5. The preparation method according to claim 1, characterized in that: The conditions of the hydrothermal reaction in step S3 are: hydrothermal temperature is 160° C., and reaction time is 12 h.
6. The preparation method according to claim 1, characterized in that: The concentration of the silver nitrate solution in step S5 is 10-100 mmol / L.
7. The preparation method according to claim 1, characterized in that: The alkaline solution in step S5 has a concentration of: 0.01-0.1 mol / L aqueous solution of NaOH, KOH or LiOH.
8. The preparation method according to claim 1, characterized in that: In step S5, the halloysite hydrothermal carbon composite material and the silver nitrate solution are mixed at a solid-liquid ratio of 1 g / 100 mL, and the amount of the alkaline solution added is a ratio of the mass of the halloysite hydrothermal carbon composite material to the volume of the alkaline solution of 1 g / 10 mL.
9. The halloysite-based composite material obtained by the preparation method according to claims 1-8, characterized in that: The halloysite-based composite material structure is that a layer of hydrothermal carbon film is covered on the surface of halloysite, and silver oxide nanoparticles are precipitated on the surface of the carbon film.
10. The halloysite-based composite material according to claim 9, characterized in that: The halloysite-based composite material is used for synchronously adsorbing radioactive iodine ions and cesium ions.
Citation Information
Patent Citations
Hydroxyl-based modified magnetic material with radionuclide adsorption function and preparation method
CN105632575A
Cesium ion removal method based on bentonite-chitosan composite microspheres
CN108428486A
Magnetic prussian blue material, preparation thereof, and applications of magnetic prussian blue material in adsorption of cesium ions
CN110327899A
Halloysite-based composite material for removing radioactive iodide ions and preparation method of halloysite-based composite material
CN113019312A
Composite carbon material and application thereof in lithium ion battery
CN114772582A