Catalyst for preparing formaldehyde from methanol as well as synthesis method and application of catalyst

The iron-molybdenum catalyst with nanostructure was prepared by co-precipitation reaction of metal compounds of molybdenum sources, cerium sources and iron sources, which solved the problem of catalyst powdering, improved selectivity and conversion, and extended the use of catalysts. life.

CN118925739APending Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411079832.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing iron-molybdenum catalysts will pulverize after the service time is extended, affecting their activity and service life. The existing technology has not fundamentally solved the catalyst life problem.

Method used

The metal compounds of molybdenum, cerium and iron sources are co-precipitated with inorganic salts. After ultrasonication, heating, aging, drying and calcination, molding catalysts with nanostructures are prepared to form a three-dimensional network structure to improve wear resistance. performance.

Benefits of technology

It improves the selectivity and conversion of the catalyst and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure HDA0004983387660000011
    Figure HDA0004983387660000011
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing formaldehyde from methanol and a synthesis method and application thereof, and the synthesis method comprises the following steps: 1) mixing a metal compound at least comprising a molybdenum source, a cerium source and an iron source with an inorganic salt as a precursor, and carrying out a coprecipitation reaction on a solution containing the dissolved precursor, the inorganic salt is one or more of sodium zirconate and lithium zirconate; (2) carrying out ultrasonic treatment and heating treatment on reaction liquid obtained after the coprecipitation reaction in the step (1) is finished; (3) aging the reaction liquid treated in the step (2) to obtain a dried solid product; and 4) carrying out molding treatment on the solid product obtained in the step 3), and roasting to obtain the molded catalyst. The catalyst prepared by the method is good in wear resistance, and the selectivity and the conversion rate of the catalyst can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to a catalyst for preparing formaldehyde from methanol, a synthesis method and application thereof. Background Art

[0002] Formaldehyde is an important basic organic chemical raw material, which plays a decisive role in the adjustment of future energy structure and the development of chemical industry. At present, my country has become the world's largest formaldehyde producer and consumer. By 2022, the domestic demand has exceeded 2800×10 4 ton.

[0003] Formaldehyde can be produced from raw materials such as methanol, dimethyl ether, and natural gas, among which methanol to formaldehyde process is the most widely used. The methanol air oxidation method is divided into the silver method and the iron-molybdenum method. Compared with the silver method, the iron-molybdenum method has a low reaction temperature and a high formaldehyde concentration, and has the advantages of low cost and high output. At present, there are some public technologies for producing formaldehyde using iron-molybdenum catalysts, such as:

[0004] For example, US4420421 describes that different raw materials, sodium molybdate, are used to achieve a methanol conversion rate of 93% to 95%, and the selectivity is increased to 92%; Patent CN105457648A prepares a catalyst containing a large number of mesopores and a certain proportion of macropores by coprecipitation, which is beneficial to the mass transfer and heat transfer of the catalyst and improves the activity of the catalyst; CN110893344A uses metallic iron, organic acid and molybdic acid as raw materials, and the iron-molybdenum catalyst prepared by coprecipitation with by-product hydrogen achieves efficient methanol conversion at 200 to 350°C, but its inlet methanol concentration is low, and the actual formaldehyde space-time yield is low.

[0005] However, the existing iron-molybdenum catalyst will be pulverized to varying degrees as the use time increases, thereby affecting the activity and service life of the catalyst. The above prior art improves the activity and selectivity of the catalyst by adding additives, but does not fundamentally solve the problem of catalyst life. Summary of the invention

[0006] In order to solve the above defects in the prior art, the present invention provides a catalyst for preparing formaldehyde from methanol, a synthesis method and application thereof. The catalyst prepared by the method of the present invention has good wear resistance and can improve the selectivity and conversion rate of the catalyst.

[0007] To achieve the above-mentioned object of the invention, the first aspect of the present invention provides a method for synthesizing a catalyst for preparing formaldehyde from methanol, comprising the following steps:

[0008] 1) mixing a metal compound including at least a molybdenum source, a cerium source and an iron source with an inorganic salt as a precursor, and subjecting a solution containing the dissolved precursor to a coprecipitation reaction, wherein the inorganic salt is one or more of sodium zirconate and lithium zirconate;

[0009] 2) subjecting the reaction solution after the coprecipitation reaction in step 1) to ultrasonic and heating treatment; the ultrasonic frequency range of the ultrasonic treatment is 30kHz to 50kHz, the temperature of the heating treatment is 30 to 80°C, and the treatment time is 0.1 to 2h;

[0010] 3) aging the reaction solution treated in step 2) to obtain a dry solid product;

[0011] 4) The solid product obtained in step 3) is shaped and calcined to obtain a shaped catalyst.

[0012] Furthermore, the molybdenum source in step 1) includes any one or a combination of at least two of ammonium polymolybdate, molybdenum trioxide, molybdic acid and molybdenum disulfide.

[0013] Furthermore, the cerium source in step 1) is cerium nitrate.

[0014] Furthermore, the iron source in step 1) includes any one of ferric chloride, ferric nitrate, ferric oxide, and iron powder, or a combination of at least two of them.

[0015] Furthermore, in step 1), the conditions for subjecting the solution containing the dissolved precursor to a coprecipitation reaction include: a pH value of the reaction solution of 1.0 to 3.0 and a temperature of 50 to 100°C.

[0016] Furthermore, the aging conditions in step 3) include: aging at 50° C. to 100° C. for 24 to 48 hours.

[0017] Furthermore, the drying conditions in step 3) include: drying at 50°C to 100°C for 10 to 28 hours, and then drying at 100°C to 150°C for 15h to 30h.

[0018] Furthermore, the molding methods described in step 4) include but are not limited to extrusion, tableting, rolling, etc.; the shapes of the obtained molded catalysts include but are not limited to strips, cylinders, hollow cylinders, spherical particles, etc.

[0019] Furthermore, the calcination conditions in step 4) include: calcination at 400°C to 560°C for 5 to 20 hours.

[0020] The second aspect of the present invention provides a methanol-to-formaldehyde catalyst prepared by the above method.

[0021] Furthermore, in the catalyst, the molar ratio of Mo / Fe is 0.5 to 1.0:1; the molar ratio of Zr / Fe is 0.1 to 2.0; and the molar ratio of Ce / Fe is 0.1 to 0.4.

[0022] The third aspect of the present invention provides the use of the catalyst or the catalyst prepared by the method in the process of methanol oxidation to formaldehyde. The reaction conditions of the catalyst in the process of methanol oxidation to formaldehyde include: reaction temperature of 320-420°C; reaction pressure of 0.05-0.3MPa absolute pressure; gas raw material volume space velocity of 7000-12000h -1 The gas raw material includes methanol, dilution gas and O2, and preferably, the dilution gas is N2.

[0023] Furthermore, the molar ratio of methanol, diluent gas and O2 is 1:9-12:1-3.

[0024] Furthermore, the catalyst is pretreated before use; preferably, the pretreatment comprises the following steps: the catalyst is heated at a volume space velocity of 5000 to 10000 h -1 In an atmosphere of air or O2 / N2 mixed gas, the temperature is raised to 200-400°C at a rate of 1-20°C / min and maintained for 30-180min. -1 N2 purge for 1 to 180 minutes.

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] The present invention mixes a metal compound including at least a molybdenum source, a cerium source and an iron source with an inorganic salt as a precursor, and performs a coprecipitation reaction on a solution containing the dissolved precursor, wherein the inorganic salt is one or more of sodium zirconate and lithium zirconate; the reaction liquid after the coprecipitation reaction is subjected to ultrasonic and heating treatment, and the precursor gradually forms a substance with a three-dimensional network structure, and then undergoes aging, drying, molding and roasting steps to finally prepare a formed catalyst with a nanostructure. The catalyst prepared by the present invention is used in the methanol oxidation process to produce formaldehyde, which can not only improve the catalyst selectivity and conversion rate, but also increase its wear resistance and extend the life of the catalyst.

[0027] Other features and advantages of the present invention will be described in detail through the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is an electron microscope image of the methanol-to-formaldehyde catalyst prepared in Example 1 of the present invention (the electron microscope instrument model is Supra55). DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The first aspect of the present invention provides a method for synthesizing a catalyst for preparing formaldehyde from methanol, comprising the following steps:

[0031] 1) mixing a metal compound including at least a molybdenum source, a cerium source and an iron source with an inorganic salt as a precursor, and subjecting a solution containing the dissolved precursor to a coprecipitation reaction, wherein the inorganic salt is one or more of sodium zirconate and lithium zirconate;

[0032] 2) subjecting the reaction solution after the coprecipitation reaction in step 1) to ultrasonic and heating treatment;

[0033] 3) aging the reaction solution treated in step 2) to obtain a dry solid product;

[0034] 4) The solid product obtained in step 3) is shaped and calcined to obtain a shaped catalyst.

[0035] The present invention mixes a metal compound including at least a molybdenum source, a cerium source and an iron source with an inorganic salt as a precursor, subjects a solution containing the dissolved precursor to a coprecipitation reaction, and subjects the reaction liquid after the coprecipitation reaction to ultrasonic and heat treatment, so that the precursor gradually forms a substance with a three-dimensional network structure. After aging, drying, molding and calcination, a formed catalyst with a nanostructure is finally prepared.

[0036] In some embodiments, the molybdenum source in step 1) includes any one or a combination of at least two of ammonium polymolybdate, molybdenum trioxide, molybdic acid and molybdenum disulfide.

[0037] In some embodiments, the cerium source in step 1) is cerium nitrate.

[0038] In some embodiments, the iron source in step 1) includes any one of ferric chloride, ferric nitrate, ferric oxide, and iron powder, or a combination of at least two thereof.

[0039] In some embodiments, the molar ratio of Mo / Fe in the molybdenum source and the iron source is 0.5 to 1.0, the molar ratio of Zr / Fe in the inorganic salt and the iron source is 0.1 to 2.0, and the molar ratio of Ce / Fe in the cerium source and the iron source is 0.1 to 0.4. When the above dosage ranges are set, the catalyst selectivity and conversion rate can be improved.

[0040] In the present invention, the various metal compounds and inorganic salts used are soluble in water or dilute acid. At the same time, when mixed and used, it should also be satisfied that no precipitation will be generated between the different components.

[0041] In some embodiments, the conditions for the coprecipitation reaction of the solution containing the dissolved precursor in step 1) include: the pH value of the reaction solution is 1.0 to 3.0, and the temperature is 50 to 100° C. Exemplarily, potassium hydroxide or sodium hydroxide is added to the reaction solution to adjust the pH value.

[0042] In some embodiments, the conditions for the ultrasonic and heating treatment in step 2) include: the ultrasonic frequency range of the ultrasonic treatment is 30kHz to 50kHz, the heating temperature is 30 to 80°C, and the treatment time is 0.1 to 2h. When the ultrasonic treatment is carried out within the above parameter range, the catalyst structure changes to form a colloid. If it is not within the above parameter range, it cannot be guaranteed that a colloid can be formed.

[0043] In some embodiments, the aging conditions in step 3) include: aging at 50° C. to 100° C. for 24 to 48 hours.

[0044] In some embodiments, the drying conditions in step 3) include: drying at 50° C. to 100° C. for 10 to 28 hours, and then drying at 100° C. to 150° C. for 15 hours to 30 hours.

[0045] In some embodiments, the molding method in step 4) includes but is not limited to extrusion, tableting, rolling, etc.; the shape of the obtained molded catalyst includes but is not limited to strips, cylinders, hollow cylinders, spherical particles, etc.

[0046] Exemplarily, a suitable extrusion molding method comprises the following steps: adding a pore-forming agent and a binder to the catalyst powder for extrusion molding to obtain strip particles. The pore-forming agent is one or more of sesbania powder, cellulose, hydroxymethyl cellulose, and polyvinyl alcohol, and the amount of the pore-forming agent is 1% to 6% of the mass of the catalyst powder. The binder is one or more of water, glycerol, ethanol, graphite, stearic acid, magnesium stearate, and zinc stearate, preferably one or more of water, glycerol, graphite, and magnesium stearate, and the amount of the binder is 8% to 15% of the mass of the catalyst powder.

[0047] Exemplarily, a suitable tableting method comprises the following steps: adding a pore-forming agent and a lubricant to the catalyst powder for tableting to obtain cylindrical or hollow cylindrical particles. The pore-forming agent is one or more of sesbania powder, cellulose, polyethylene, polypropylene, and polyvinyl chloride, preferably sesbania powder and / or cellulose, and the amount of the pore-forming agent is 1% to 5% of the mass of the catalyst powder. The lubricant is one or more of stearic acid, magnesium stearate, zinc stearate, and graphite, preferably one or more of magnesium stearate, zinc stearate, and graphite, and the amount of the lubricant is 0.1% to 1% of the mass of the catalyst powder.

[0048] Exemplarily, a suitable rolling forming method comprises the following steps: adding a pore-forming agent and a binder to the catalyst powder, and rolling forming with a spherical carrier. The pore-forming agent is one or more of sesbania powder, cellulose, polyvinyl alcohol, polyvinyl pyrrolidone, starch, and pullulan, preferably one or more of sesbania powder, polyvinyl pyrrolidone and starch, and the amount of the pore-forming agent is 1% to 5% of the mass of the catalyst powder. The binder is one or more of water, ethanol, ethylene glycol, and glycerol, preferably one or more of water, ethanol and glycerol, and the amount of the binder is 20% to 35% of the catalyst powder. The spherical carrier is preferably a porous alumina carrier with a diameter of 2.3 to 3.5 mm, and the amount is 50% to 70% of the mass of the catalyst powder.

[0049] In some embodiments, the calcination conditions in step 4) include: calcination at 400° C. to 560° C. for 5 to 20 hours.

[0050] The second aspect of the present invention provides a methanol-to-formaldehyde catalyst prepared by the above method.

[0051] In some embodiments, in the catalyst, the Mo / Fe molar ratio is 0.5-1.0:1; the Zr / Fe molar ratio is 0.1-2.0; and the Ce / Fe molar ratio is 0.1-0.4.

[0052] The third aspect of the present invention provides the use of the catalyst or the catalyst obtained by the method in the process of methanol oxidation to formaldehyde. The reaction conditions of the catalyst in the process of methanol oxidation to formaldehyde conversion include: reaction temperature of 320-420°C; reaction pressure of 0.05-0.3MPa absolute pressure; gas raw material volume space velocity of 7000-12000h -1 The gas raw material includes methanol, dilution gas and O2, and preferably, the dilution gas is N2.

[0053] In some embodiments, the molar ratio of methanol, diluent gas and O2 is 1:9-12:1-3.

[0054] In some embodiments, the catalyst is pretreated before use; preferably, the pretreatment comprises the following steps: the catalyst is heated at a volume space velocity of 5000 to 10000 h -1 In an atmosphere of air or O2 / N2 mixed gas, the temperature is raised to 200-400°C at a rate of 1-20°C / min and maintained for 30-180min. -1 N2 purge for 1 to 180 minutes.

[0055] The following are typical but non-limiting embodiments of the present invention:

[0056] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0057] In the following examples, the reaction outlet gas was effectively captured, and the product analysis was performed by gas chromatography and liquid chromatography GC-2014. The conversion rate of methanol and the formaldehyde selectivity were calculated by the following formula:

[0058]

[0059] Example 1

[0060] Dissolve 0.07 mol of ammonium heptamolybdate (chemical formula: (NH4)6Mo7O2·4H2O), 1 mol of ferric chloride hexahydrate (chemical formula: FeCl3·6H2O), 0.1 mol of cerium nitrate (chemical formula: Ce(NO3)3), and 0.1 mol of sodium zirconate in 1000 g of deionized water, stir well, and add them into the reactor in a stream, keeping the solution temperature in the reactor at 90°C, and add 0.11 mol of sodium hydroxide to adjust the pH value to 2.0 for co-precipitation.

[0061] The reaction solution was subjected to ultrasonic treatment (Merritek Technology, model UC-6200, 40kHz, 30°C) for 1.5h, and then kept at 90°C for 28h after ultrasonic treatment. After filtration and washing, the filter cake was dried at 90°C for 24h and then at 120°C for 20h. After drying, a block solid was obtained, which was crushed to obtain particles of 30-60 mesh.

[0062] Take 50g of 30-60 mesh granules, add 2.5g of pore-forming agent sesbania powder and 0.5g of lubricant magnesium stearate, mix well, and form into hollow cylindrical granules by tablet press. The formed granules are calcined at 420°C for 5h to obtain a catalyst.

[0063] 25g of catalyst was loaded into a 50cm long reactor, where the reaction tube was a 25mm stainless steel reaction tube. The catalyst pretreatment process was as follows: firstly, air was introduced at a volume space velocity of 8000h-1 The temperature of the reaction tube was heated from room temperature to 250°C at a heating rate of 5°C / min and maintained for 120 min, then switched to nitrogen purge for 180 min at a purge volume space velocity of 2000 h -1 .

[0064] After the catalyst pretreatment was completed, methanol: oxygen: nitrogen: water = 1:1.3:10:0.13 (molar ratio), volume space velocity 10000h -1 The oxidation reaction was carried out under the conditions of (standard state), temperature of 380°C and normal pressure for 100 hours. The selectivity of formaldehyde was 98.5% and the conversion rate of methanol was 98.8%.

[0065] Figure 1 This is an electron microscope image of the methanol to formaldehyde catalyst prepared in Example 1 of the present invention. It can be seen from the image that the catalyst prepared in the present invention forms a three-dimensional network structure. This special structure can improve the catalyst's wear resistance while improving the catalyst's selectivity and conversion rate.

[0066] The catalyst is divided into four layers from the inside to the outside, and the particle sizes of each layer are 32, 18, 12, and 3 (in microns).

[0067] Example 2

[0068] Dissolve 0.1 mol of ammonium heptamolybdate (chemical formula: (NH4)6Mo7O2·4H2O), 1 mol of ferric chloride hexahydrate (chemical formula: FeCl3·6H2O), 0.2 mol of cerium nitrate (chemical formula: Ce(NO3)3), and 1.5 mol of sodium zirconate in 1000 g of deionized water, stir well, and add into the reactor, keep the solution temperature in the reactor at 90°C, and add 0.15 mol of sodium hydroxide to adjust the pH value to 2.0 for coprecipitation.

[0069] The reaction solution was subjected to ultrasonic treatment for 1.5 h (Merritek Technology, model UC-6200, 40 kHz, 30°C), and maintained at 90°C for 28 h after ultrasonic treatment. Filter and wash, and the filter cake was dried at 90°C for 24 h and then at 120°C for 20 h. After drying, a block solid was obtained, which was crushed to obtain particles of 30 to 60 mesh.

[0070] Take 50g of 30-60 mesh granules, add 2.5g of pore-forming agent sesbania powder and 0.5g of lubricant magnesium stearate, mix well, and form into hollow cylindrical granules by tablet press. The formed granules are calcined at 420°C for 5h to obtain a catalyst.

[0071] 25g of catalyst was loaded into a 50cm long reactor, where the reaction tube was a 25mm stainless steel reaction tube. The catalyst pretreatment process was as follows: firstly, air was introduced at a volume space velocity of 8000h -1The temperature of the reaction tube was heated from room temperature to 250°C at a heating rate of 5°C / min and maintained for 120 min, then switched to nitrogen purge for 180 min at a purge volume space velocity of 3000 h -1 .

[0072] After the catalyst pretreatment was completed, methanol: oxygen: nitrogen: water = 1:1.3:10:0.13 (molar ratio), volume space velocity 10000h -1 The oxidation reaction was carried out under the conditions of (standard state), temperature of 380°C and normal pressure for 100 hours. The selectivity of formaldehyde was 95.0% and the conversion rate of methanol was 98.8%.

[0073] Example 3

[0074] Dissolve 0.14 mol of ammonium heptamolybdate (chemical formula: (NH4)6Mo7O2·4H2O), 1 mol of ferric chloride hexahydrate (chemical formula: FeCl3·6H2O), 0.4 mol of cerium nitrate (chemical formula: Ce(NO3)3, and 2 mol of sodium zirconate in 1000 g of deionized water, stir well, and add them into the reactor. Keep the temperature of the solution in the reactor at 90°C, add 0.18 mol of sodium hydroxide to adjust the pH value to 2.0 for coprecipitation.

[0075] The reaction solution was subjected to ultrasonic treatment for 1.5 h (Merritek Technology, model UC-6200, 40 kHz, 30°C), and maintained at 90°C for 28 h after ultrasonic treatment. Filter and wash, and the filter cake was dried at 90°C for 24 h and then at 120°C for 20 h. After drying, a block solid was obtained, which was crushed to obtain particles of 30 to 60 mesh.

[0076] Take 50g of 30-60 mesh granules, add 2.5g of pore-forming agent sesbania powder and 0.5g of lubricant magnesium stearate, mix well, and form into hollow cylindrical granules by tablet press. The formed granules are calcined at 420°C for 5h to obtain a catalyst.

[0077] 25g of catalyst was loaded into a 50cm long reactor, where the reaction tube was a 25mm stainless steel reaction tube. The catalyst pretreatment process was as follows: firstly, air was introduced at a volume space velocity of 8000h -1 The temperature of the reaction tube was heated from room temperature to 250°C at a heating rate of 5°C / min and maintained for 120 min, then switched to nitrogen purge for 180 min at a purge volume space velocity of 2000 h -1 .

[0078] After the catalyst pretreatment was completed, methanol: oxygen: nitrogen: water = 1:1.3:10:0.13 (molar ratio), volume space velocity 10000h -1The oxidation reaction was carried out under the conditions of (standard state), temperature of 380°C and normal pressure for 100 hours. The selectivity of formaldehyde was 94.5% and the conversion rate of methanol was 98.1%.

[0079] Example 4

[0080] The difference from Example 1 is that: at 35 kHz, the ultrasonic temperature is 60° C., the ultrasonic wave is applied for 2 hours, and the catalyst is subjected to oxidation reaction for 100 hours in the same manner as in Example 1, and the formaldehyde selectivity and methanol conversion rate are 95.1% and 98.9% respectively.

[0081] Example 5

[0082] The difference from Example 1 is that: at 20 kHz, the ultrasonic temperature is 80° C., the ultrasonic wave is applied for 1 hour, and the catalyst is subjected to oxidation reaction for 100 hours in the same manner as in Example 1, and the formaldehyde selectivity and methanol conversion rate are 95.5% and 97.9% respectively.

[0083] Example 6

[0084] The difference from Example 1 is that 0.1 mol lithium zirconate is added and dissolved in 1 L, 0.1 mol\L dilute sulfuric acid, and the catalyst is subjected to oxidation reaction for 100 h in the same manner as in Example 1, and the formaldehyde selectivity and methanol conversion rate are 94.8% and 98.6%, respectively.

[0085] Comparative Example 1

[0086] Dissolve 0.07mol of ammonium heptamolybdate (chemical formula: (NH4)6Mo7O2·4H2O), 1mol of ferric chloride hexahydrate (chemical formula: FeCl3·6H2O), and 0.1mol of cerium nitrate (chemical formula: Ce(NO3)3) in 1000g of deionized water, stir well, and add them to the reactor in a stream, keep the temperature of the solution in the reactor at 90℃, add 0.1mol of sodium hydroxide to adjust the pH value to 2.0 for coprecipitation, and then keep 90℃ for stirring and aging for 28h. Filter and wash, dry the filter cake at 90℃ for 24h and then at 120℃ for 20h. After drying, a block solid is obtained, which is crushed to obtain 30-60 mesh particles. Take 50g of 30-60 mesh particles, add 2.5g of pore-forming agent sesbania powder and 0.5g of lubricant magnesium stearate, mix well, and use a tablet press to form hollow cylindrical particles. The formed particles are roasted at 420℃ for 5h to obtain a catalyst.

[0087] The oxidation reaction was carried out for 100 hours in the same manner as in Example 1. The selectivity of formaldehyde was 90.5%, and the conversion rate of methanol was 92.8%. Comparative Example 1 was different from Example 1 in that sodium zirconate was not added and ultrasonic treatment was not performed, resulting in reduced formaldehyde selectivity and methanol conversion rate.

[0088] Comparative Example 2

[0089] 0.07 mol of ammonium heptamolybdate (chemical formula: (NH4)6Mo7O2·4H2O), 1 mol of ferric chloride hexahydrate (chemical formula: FeCl3·6H2O), and 0.1 mol of cerium nitrate (chemical formula: Ce(NO3)3) were dissolved in 1000 g of deionized water, stirred thoroughly, and added into the reactor in a stream, while maintaining the solution temperature at 90°C. 0.1 mol of sodium hydroxide was added to adjust the pH value to 2.0 for co-precipitation.

[0090] The reaction solution was subjected to ultrasonic treatment for 1.5 h (Merritek Technology, model UC-6200, 40 kHz, 30°C), and maintained at 90°C for 28 h after ultrasonic treatment. Filter and wash, and the filter cake was dried at 90°C for 24 h and then at 120°C for 20 h. After drying, a block solid was obtained, which was crushed to obtain particles of 30 to 60 mesh.

[0091] Take 50g of 30-60 mesh granules, add 2.5g of pore-forming agent sesbania powder and 0.5g of lubricant magnesium stearate, mix well, and form into hollow cylindrical granules by tablet press. The formed granules are calcined at 420°C for 5h to obtain a catalyst.

[0092] The oxidation reaction was carried out for 100 hours in the same manner as in Example 1. The selectivity of formaldehyde was 92.5%, and the conversion rate of methanol was 93.8%. Comparative Example 2 was different from Example 1 in that sodium zirconate was not added, which reduced the selectivity of formaldehyde and the conversion rate of methanol.

[0093] Comparative Example 3

[0094] Dissolve 0.07mol of ammonium heptamolybdate (chemical formula: (NH4)6Mo7O2·4H2O), 1mol of ferric chloride hexahydrate (chemical formula: FeCl3·6H2O), 0.1mol of cerium nitrate (chemical formula: Ce(NO3)3), and 0.1mol of sodium zirconate in 1000g of deionized water, stir well, and add them to the reactor in parallel. Keep the temperature of the solution in the reactor at 90℃, add 0.1mol of sodium hydroxide to adjust the pH value to 2.0 for coprecipitation, and then keep 90℃ for stirring and aging for 28h. Filter and wash, dry the filter cake at 90℃ for 24h and then at 120℃ for 20h. After drying, a block solid is obtained, which is crushed to obtain 30-60 mesh particles. Take 50g of 30-60 mesh particles, add 2.5g of pore-forming agent sesbania powder and 0.5g of lubricant magnesium stearate, mix well, and use a tablet press to form hollow cylindrical particles. The formed particles were calcined at 420°C for 5 h to obtain a catalyst.

[0095] The oxidation reaction was carried out for 100 hours in the same manner as in Example 1. The selectivity of formaldehyde was 91.5% and the conversion rate of methanol was 93.8%. Comparative Example 3 was different from Example 1 in that sodium zirconate was added but ultrasonic treatment was not performed, which reduced the selectivity of formaldehyde and the conversion rate of methanol.

[0096] By comparing Example 1 with Comparative Examples 1, 2 and 3, it can be seen that the catalyst selectivity and conversion rate can be improved by adding inorganic salts and adopting ultrasonic heating to prepare the catalyst, and its wear resistance can be increased and the life of the catalyst can be extended.

[0097] Comparative Example 4

[0098] The difference from Example 1 is that 0.1 mol of zirconium chloride is added, and the catalyst is subjected to 100 h oxidation reaction in the same manner as in Example 1; the selectivity of formaldehyde is 91.3%, and the conversion rate of methanol is 90.5%. The difference from Example 1 in Comparative Example 4 is that the added inorganic salt is inappropriate and cannot form a colloid, which reduces the selectivity of formaldehyde and the conversion rate of methanol.

[0099] Comparative Example 5

[0100] The difference from Example 1 is that the ultrasonic temperature is 60°C for 5 hours, and the catalyst is subjected to oxidation reaction for 100 hours in the same manner as in Example 1. The formaldehyde selectivity is 91.5%, and the methanol conversion rate is 93.8%. The formaldehyde selectivity and methanol conversion rate are lower than those in Example 1. The difference between Comparative Example 5 and Example 1 is that the ultrasonic time is not appropriate, and a colloid cannot be formed, which reduces the formaldehyde selectivity and methanol conversion rate.

[0101] Obviously, the above embodiments of the present invention are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are within the spirit scope of the present invention.

Claims

1. A method for synthesizing a catalyst for preparing formaldehyde from methanol, characterized in that: The steps include: 1) mixing a metal compound including at least a molybdenum source, a cerium source and an iron source with an inorganic salt as a precursor, and subjecting a solution containing the dissolved precursor to a coprecipitation reaction, wherein the inorganic salt is one or more of sodium zirconate and lithium zirconate; 2) subjecting the reaction solution after the coprecipitation reaction in step 1) to ultrasonic and heating treatment; the ultrasonic frequency range of the ultrasonic treatment is 30kHz to 50kHz, the temperature of the heating treatment is 30 to 80°C, and the treatment time is 0.1 to 2h; 3) aging the reaction solution treated in step 2) to obtain a dry solid product; 4) The solid product obtained in step 3) is shaped and calcined to obtain a shaped catalyst.

2. The method for synthesizing the catalyst according to claim 1, characterized in that: Step 1) the metal compound comprises any one of a soluble salt of the corresponding metal, a metal oxide, a metal element or a combination of at least two thereof; The molybdenum source in step 1) comprises any one or a combination of at least two of ammonium polymolybdate, molybdenum trioxide, molybdic acid and molybdenum disulfide; The cerium source in step 1) is cerium nitrate; The iron source in step 1) includes any one of ferric chloride, ferric nitrate, ferric oxide, and iron powder, or a combination of at least two of them.

3. The method for synthesizing the catalyst according to claim 1 or 2, characterized in that: Step 1) The conditions for subjecting the solution containing the dissolved precursor to a coprecipitation reaction include: the pH value of the reaction solution is 1.0 to 3.0, and the temperature is 50 to 100°C.

4. The method for synthesizing the catalyst according to claim 1, characterized in that: Step 3) The aging conditions include: aging at 50° C. to 100° C. for 24 to 48 hours.

5. The method for synthesizing the catalyst according to claim 1, characterized in that: Step 3) The drying conditions include: drying at 50°C to 100°C for 10 to 28 hours, and then drying at 100°C to 150°C for 15h to 30h.

6. The method for synthesizing the catalyst according to claim 1, characterized in that: Step 4) The molding method includes but is not limited to extrusion, tableting, and rolling; the shape of the obtained molded catalyst includes but is not limited to strips, cylinders, hollow cylinders, and spherical particles; and / or, Step 4) The calcination conditions include: calcining at 400°C to 560°C for 5 to 20 hours.

7. A methanol to formaldehyde catalyst prepared by the method according to any one of claims 1 to 6.

8. The catalyst according to claim 7, characterized in that In the catalyst, the molar ratio of Mo / Fe is 0.5-1.0:1, the molar ratio of Zr / Fe is 0.1-2.0, and the molar ratio of Ce / Fe is 0.1-0.

4.

9. Use of the catalyst prepared by the method according to any one of claims 1 to 6 or the catalyst according to any one of claims 7 to 8 in a process of producing formaldehyde by oxidation of methanol, characterized in that: The reaction conditions of the catalyst in the process of methanol oxidation to formaldehyde include: reaction temperature of 320-420°C; reaction pressure of 0.05-0.3 MPa absolute pressure; gas raw material volume space velocity of 7000-12000 h -1 The gas raw material includes methanol, diluent gas and O2. Preferably, the diluent gas is N2, and the molar ratio of methanol, diluent gas and O2 is 1:9-12:1-3.

10. Use of the catalyst according to claim 9 in a process for producing formaldehyde by oxidation of methanol, characterized in that: The catalyst is pretreated before use; the pretreatment comprises the following steps: Catalyst at volume space velocity 5000~10000h -1 In an atmosphere of air or O2 / N2 mixed gas, the temperature is raised to 200-400°C at a rate of 1-20°C / min and maintained for 30-180min. -1 N2 purge for 1 to 180 minutes.