Solid acid catalyst and preparation method of galactose

By using porous skeleton solid acid catalyst formed by crosslinking ferric oxide silicon atoms and antimony oxide in galactose preparation, the problem of difficulty in recycling liquid acid catalysts and environmental pollution is solved, and efficient catalytic and recyclable solid acids are achieved. Catalytic effect.

CN118925747AInactive Publication Date: 2024-11-12SYNGARS TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411427984.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional liquid acid catalysts have problems of recycling difficulties, environmental pollution and high production costs in the preparation of galactose, and their use will generate harmful wastewater and waste gases, threatening human health.

Method used

The crosslinked silicon atoms of iron trioxide and antimony oxide are mixed into the porous framework to form a solid acid catalyst with stable structure. Through the mixing of iron sulfate and silicon oxide and the mutual melting of antimony oxide, SiO2/Sb2O3/Fe2O3-SO3 solid is formed. Acid is used to support sulfate to increase catalytic rate.

Benefits of technology

The efficient catalysis of galactose is achieved, which significantly improves the catalytic rate and separation rate. At the same time, solid acid catalysts can be recycled and reused, reducing environmental pollution and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925747A_ABST
    Figure CN118925747A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a solid acid catalyst. The preparation method comprises the following steps: S1, dissolving Fe2O3 in sulfuric acid; s2, adding solid-phase SiO2 into the ferric sulfate solution obtained in the step S1, and heating the solid-phase SiO2 and Fe2 (SO4) 3 solution under rotary stirring; in the heating process, Fe2 (SO4) 3 reacts with water to generate Fe2O3 and sulfuric acid; under the condition of constant temperature, Fe2O3 / SiO2-SO3 is formed; s3, solid Sb2O3 is added, rotary stirring is conducted, the temperature is increased till the mixture is mutually fused, and solid acid is obtained; s4, calcining to obtain a target solid acid catalyst; the prepared solid acid catalyst is used for preparing galactose, lactose is used as a raw material, the SiO2 / Sb2O3 / Fe2O3-SO3 solid acid catalyst is used, the structure is stable, effective separation is achieved through direct filtration, the separated and recycled solid acid catalyst can be recycled, activated and repeatedly used, and the catalytic efficiency is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of galactose preparation, and in particular to a solid acid catalyst and a method for preparing galactose. Background Art

[0002] In the fields of organic chemistry, catalytic reactions, and carbohydrate chemistry, galactose is an important monosaccharide widely used in food, medicine, chemical industry, and other industries. The traditional galactose preparation process mainly uses liquid acid catalysts, such as sulfuric acid, hydrochloric acid, etc. Although these catalysts can effectively catalyze the reaction, they have problems such as difficult recycling, serious environmental pollution, and high production costs. In addition, the use of liquid acid catalysts is also accompanied by the generation of harmful wastewater and waste gas, which will further threaten human health. In order to cooperate with the use and recovery of liquid acid catalysts, a large amount of solvents and auxiliary materials are also required for use.

[0003] For example, Chinese invention patent CN108726766B discloses a method for treating catalyst production wastewater, wherein the catalyst production wastewater contains NH 4+ 、SO 4 2- , Cl - and Na + , after adjusting the pH value of the wastewater to be treated to a specific range in advance, the MVR evaporation device is used for evaporation separation to obtain a concentrated solution containing sodium sulfate crystals and sodium chloride crystals and a relatively concentrated ammonia water, and then the sodium sulfate in the concentrated solution is dissolved by low temperature treatment, and the sodium chloride is further crystallized to obtain sodium chloride crystals. Then, the multi-effect evaporation device is used for evaporation again to obtain a concentrated solution containing sodium sulfate crystals and a relatively dilute ammonia water to obtain sodium sulfate crystals. This method can obtain high-purity sodium chloride and sodium sulfate respectively, avoiding the difficulties in mixed salt treatment and reuse, and completing the process of separating ammonia and salt at the same time, and using heat exchange to heat up the wastewater and cool down the ammonia-containing steam at the same time, reasonably utilizing the heat in the evaporation process, saving energy, and reducing the cost of wastewater treatment. The ammonium in the wastewater is recovered in the form of ammonia water, and the sodium sulfate and sodium chloride are recovered in the form of crystals respectively. It can be seen that the recovery of liquid phase catalysts is difficult and the recovery cost is high, which is not conducive to environmental protection. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a solid acid catalyst. The present invention uses ferric oxide to crosslink silicon atoms and mixes Sb 2 O 3 A porous skeleton for loading sulfate is prepared, and a solid acid with a stable structure is prepared, which effectively improves the catalytic rate of galactose.

[0005] To solve this technical problem, the technical solution of the present invention is: a method for preparing a solid acid catalyst, comprising the following steps: S1, Fe 2 O 3 Dissolves in sulfuric acid to form Fe 2 (SO 4 ) 3 Solution; S2, solid phase SiO 2 Add the ferric sulfate solution obtained in step S1, the solid phase SiO 2 and Fe 2 (SO 4 ) 3 The solution was heated to Fe 2 (SO 4 ) 3 Reacts with water to form Fe 2 O 3 and sulfuric acid; under constant temperature conditions, the Fe 2 O 3 With SiO 2 While mixing, sulfuric acid and Fe 2 O 3 / SiO 2 Formation of Fe 2 O 3 / SiO 2 -SO 3 Solid acid; S3, to the SiO obtained in step S2 2 / Fe 2 O 3 -SO 3 Solid acid added to solid Sb 2 O 3 , rotating and stirring, heating until the mixture is molten, Fe 2 O 3 、SiO 2 and Sb 2 O 3 Mix together to obtain SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 Solid acid; S4, calcining to obtain the target solid acid catalyst.

[0006] Preferred Fe in S1 2 O 3 The molar ratio of sulfuric acid to S1 is 1:(3.5 to 3.8). Sulfuric acid is added to dissolve a certain amount of Fe 2 O 3 , combined with the addition of silicon oxide to S2, using silicon oxide as a skeleton to effectively disperse the Fe that forms an acid center with sulfate 2 O3 The mechanism of iron oxide loaded with sulfate to form solid acid is that sulfate is coordinated and adsorbed on the surface of iron oxide, causing the electron cloud intensity on the Fe-O bond to shift and increasing the generation of L-acid centers; with subsequent drying and calcination, the structural water in the catalyst undergoes dissociative adsorption to produce proton acid.

[0007] Preferred Fe in S2 2 O 3 With SiO 2 The molar ratio is 1: (0.3 to 0.5). In the present invention, silicon oxide is used as a skeleton for loading and dispersing iron oxide. Iron oxide and silicon oxide are mixed at high temperature, and iron, silicon and oxygen form a cross structure, thereby stabilizing the structure and improving the dispersion of iron oxide.

[0008] Preferably, the constant temperature in step S2 is 337°C; the heating rate is 5°C / min to 10°C / min. During the heating process, iron sulfate and water first form iron oxide and sulfuric acid, and the regenerated iron oxide is mixed with silicon oxide. At its boiling temperature, sulfuric acid is more likely to adsorb oxides to form SiO 2 / Fe 2 O 3 -SO 3 ; The acid used in the present invention is in excess to ensure that the obtained product is fully loaded with sulfate.

[0009] Preferably, Fe 2 O 3 、SiO 2 and Sb 2 O 3 The temperature of the melting is 700℃, the heating rate is 5℃ / min to 10℃ / min, and the nitrogen is used for protection. At 700℃, the three oxides are mixed and melted, and the outermost electrons intersect to obtain SiO 2 / Fe 2 O 3 / Sb 2 O 3 In step S2, the sulfate adsorbed on the surface of the iron oxide is present on the SiO 2 / Fe 2 O 3 / Sb 2 O 3 In the structure, direct fusion of antimony trioxide and sulfuric acid is avoided, and at the same time the pore size and specific surface area of ​​the obtained solid acid catalyst are effectively improved.

[0010] Preferably, Fe 2 O 3 With Sb 2 O 3 The molar ratio is 1:(0.1 to 0.3).

[0011] Preferably, the SiO obtained in step S3 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The solid acid is immersed in sulfuric acid, stirred and immersed at low temperature, and filtered to obtain solid acid supplemented with sulfate. The high temperature in step S3 will cause part of the sulfate to be lost, so SiO 2 / Fe 2 O 3 / Sb 2 O 3 -SO 3 It is necessary to immerse in sulfuric acid at low temperature again to replenish sulfate ions to avoid Sb 2 O 3 The solid acid catalyst is reacted with acid, thereby fully utilizing the porous and structurally stable characteristics of the solid acid catalyst obtained by the invention in the preparation process of galactose.

[0012] Another object of the present invention is to provide a method for preparing galactose using the solid acid catalyst prepared by the present invention. The present invention uses lactose as a raw material and uses SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The solid acid catalyst has a stable structure and can be effectively separated by direct filtration. The solid acid catalyst prepared by the invention can be recycled and activated, can be used repeatedly, and has a stable catalytic efficiency.

[0013] To solve this technical problem, the technical solution of the present invention is: a method for preparing galactose using the solid acid catalyst prepared by the present invention, wherein lactose and the solid acid catalyst are added to a reaction container for reaction; after the reaction is completed, the solid acid catalyst is filtered to obtain a galactose conversion liquid.

[0014] SiO is preferred 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The activation method of the solid acid catalyst comprises the following steps: S11, adding the filtered and recovered solid acid catalyst into 68% sulfuric acid, soaking at low temperature, and shaking; S12, Filtration of SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3Solid acid; S13, calcined at 300℃ to obtain SiO2 that can be added to lactose 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 Solid acid catalyst.

[0015] The present invention reduces the catalytic efficiency of SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The solid acid catalyst is put back into the sulfuric acid solution to adsorb sulfate ions using Fe-O bonds, thereby being reactivated into a solid acid catalyst with high catalytic efficiency.

[0016] By adopting the above technical solution, the beneficial effects of the present invention are: The present invention provides a SiO2 catalyst for catalyzing the conversion of lactose into galactose. 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The preparation method of solid acid catalyst comprises the following steps: firstly 2 O 3 Dissolves in sulfuric acid to form Fe 2 (SO 4 ) 3 solution, and then under heating conditions, Fe 2 (SO 4 ) 3 Reacts with water to form Fe 2 O 3 , the generated Fe 2 O 3 With SiO 2 Mixing, sulfuric acid with Fe 2 O 3 With SiO 2 Formation of SiO by solid-state reaction 2 / Fe 2 O 3 -SO 3 Solid acid; then to SiO 2 / Fe 2 O 3 -SO 3 Solid acid added to solid Sb 2 O 3 , rotating and stirring, heating until the mixture is molten, Fe 2 O 3 、SiO2 and Sb 2 O 3 The outermost electrons of the three oxides intersect to obtain SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 Solid acid; the solid acid catalyst obtained by the present invention is SiO 2 / Sb 2 O 3 / Fe 2 O 3 As carrier, Fe 2 O 3 Silicon is used for coordination and adsorption of sulfate, and has a cross-linking effect, and iron, silicon and oxygen form a cross-structure, thereby stabilizing the structure and improving the dispersion of iron oxide. Antimony has a large molecular radius, and antimony trioxide is mixed into the carrier to obtain a carrier with large porosity, which is more conducive to loading acid radicals. Therefore, the solid acid catalyst obtained by the present invention has a stable structure and strong acidity, and is applied to the production of galactose prepared from lactose as a raw material, making full use of the superacid properties of the solid acid catalyst, and coordinating the porous structure and large specific surface area of ​​the obtained solid acid catalyst to effectively improve the solid-liquid contact area, so the conversion efficiency is significantly improved, and the separation rate is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Fe is the Fe used by S1 in Example 1 to form ferric sulfate with sulfuric acid 2 O 3 XRD pattern of Figure 2 Add Sb to S3 in Example 1 2 O 3 XRD pattern of Figure 3 Prepare SiO for Example 1 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 XRD patterns of solid acid catalysts. DETAILED DESCRIPTION

[0018] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0019] Example 1 This embodiment discloses a method for preparing a solid acid catalyst, comprising the following steps: S1, Fe 2 O 3Dissolved in 68% sulfuric acid to form Fe 2 (SO 4 ) 3 Solution; Fe in S1 2 O 3 The molar ratio with sulfuric acid is 1:3.5; S2, solid phase SiO 2 Add the ferric sulfate solution obtained in step S1, the solid phase SiO 2 and Fe 2 (SO 4 ) 3 The solution was heated under rotary stirring at 1 r / s and the temperature was raised to 337°C at a rate of 5°C / min. During the heating process, Fe 2 (SO 4 ) 3 Reacts with water to form Fe 2 O 3 and sulfuric acid; Fe generated under constant temperature 2 O 3 With SiO 2 Mixing, sulfuric acid and Fe 2 O 3 / SiO 2 Formation of Fe 2 O 3 / SiO 2 -SO 3 Solid acid; Fe in S2 2 O 3 With SiO 2 The molar ratio is 1:0.3.

[0020] At the boiling point of sulfuric acid, the combination of sulfonic acid groups and iron oxide is effectively enhanced, and sulfate groups are coordinated and adsorbed on the surface, causing the electron cloud intensity on the Fe-O bond to shift, increasing the generation of L-acid centers; during drying and calcination, the structural water in the catalyst undergoes dissociative adsorption to produce proton acid centers.

[0021] S3, to the SiO obtained in step S2 2 / Fe 2 O 3 -SO 3 Solid acid added to solid Sb 2 O 3 , the stirring parameter is 3r / s, the temperature is raised until the mixture is molten, Fe 2 O 3 、SiO 2 and Sb 2 O 3 Mix together to obtain SiO 2 / Sb2 O 3 / Fe 2 O 3 -SO 3 Solid acid; In step S3, Fe 2 O 3 With Sb 2 O 3 The molar ratio is 1:0.10.

[0022] In step S3, Fe 2 O 3 、SiO 2 and Sb 2 O 3 The insulation temperature for mutual melting is 700℃, the heating rate is 5℃ / min to 10℃ / min, and the nitrogen atmosphere is protected. After the reaction is completed, the mixture is kept rotating and stirred until it reaches room temperature; a higher insulation temperature is likely to cause the sulfate to be lost in the form of gaseous sulfur dioxide. Therefore, in order to ensure the number of acid centers of the solid superacid, a process step of supplementing sulfate is subsequently performed.

[0023] The SiO obtained in step S3 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The solid acid is immersed in sulfuric acid with a mass fraction of 68%, and is stirred and immersed at a low temperature of 5° C. to 10° C. for 2 hours, and the solid acid supplemented with sulfate is obtained by filtering.

[0024] S4. Calcinate at 300°C to obtain the target solid acid catalyst.

[0025] Take the XRD spectrum of iron oxide in the raw material of this embodiment, the specific spectrum is as follows Figure 1 As shown; the silicon oxide used in this embodiment is amorphous silicon oxide, so the silicon oxide is not characterized here; the XRD spectrum of antimony trioxide used in this embodiment is as shown Figure 2 As shown; SiO prepared in this embodiment 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The XRD spectrum of the solid acid catalyst is shown in Figure 3 As shown, from Figure 3 It can be seen that SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3The solid acid catalyst has diffraction peaks on different crystal faces, which shows that this example successfully composited SiO 2 / Sb 2 O 3 / Fe 2 O 3 .

[0026] The SiO prepared in this example 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The solid acid catalyst is used in the preparation of galactose, and the specific method is as follows: Lactose and the solid acid were added into the reactor in a mass ratio of 1:0.1 to react for 3 hours; after the reaction, the solid acid catalyst was filtered to obtain a galactose conversion solution.

[0027] Example 2 The main differences between this embodiment and embodiment 1 are shown in Table 1.

[0028] Example 3 The main differences between this embodiment and embodiment 1 are shown in Table 1.

[0029] Example 4 The main differences between this embodiment and embodiment 1 are shown in Table 1.

[0030] Example 5 The main differences between this embodiment and embodiment 1 are shown in Table 1.

[0031] Comparative Example 1 This comparative example discloses a method for preparing galactose using liquid sulfuric acid as a catalyst, wherein lactose and the solid acid are added to a reactor at a mass ratio of 1:0.1 and reacted for 3 hours to obtain a galactose conversion liquid.

[0032] Comparative Example 2 This comparative example discloses Fe 2 O 3 -SO 3 The preparation method of the solid acid catalyst is as follows: S1, Fe 2 O 3 Dissolves in sulfuric acid to form Fe 2 (SO 4 ) 3 Solution, Fe 2 O 3 The molar ratio with sulfuric acid is 1:3.5; The temperature was raised to 337°C at a rate of 5°C / min, and the stirring condition was 1r / s. The Fe 2O 3 -SO 3 Solid acid catalyst.

[0033] This comparative example is made of Fe 2 O 3 -SO 3 The method for preparing galactose using a solid acid catalyst is as follows: Lactose and Fe 2 O 3 -SO 3 The solid acid catalyst was added into the reactor at a mass ratio of 1:0.1 and reacted for 3 hours to obtain a galactose conversion solution.

[0034] Comparative Example 3 This comparative example discloses Fe 2 O 3 / SiO 2 -SO 3 The preparation method of the solid acid catalyst is as follows: S1, Fe 2 O 3 Soluble in H 2 SO 4 Formation of Fe 2 (SO 4 ) 3 Solution; Fe in S1 2 O 3 The molar ratio with sulfuric acid is 1:3.5; S2, solid phase SiO 2 Add the ferric sulfate solution obtained in step S1, the solid phase SiO 2 and Fe 2 (SO 4 ) 3 The solution was heated under rotary stirring at 1 r / s and the temperature was raised to 337°C at a rate of 5°C / min. During the heating process, Fe 2 (SO 4 ) 3 Reacts with water to form Fe 2 O 3 and sulfuric acid; Fe generated under constant temperature 2 O 3 With SiO 2 Mixing, sulfuric acid and Fe 2 O 3 / SiO 2 Formation of Fe 2 O 3 / SiO 2 -SO 3 Solid acid; Fe in S22 O 3 With SiO 2 The molar ratio is 1:0.3.

[0035] This comparative example is made of Fe 2 O 3 / SiO 2- SO 3 The method for preparing galactose using a solid acid catalyst is as follows: Lactose and Fe 2 O 3 / SiO 2 -SO 3 The solid acid catalyst was added into the reactor at a mass ratio of 1:0.1 and reacted for 3 hours to obtain a galactose conversion solution.

[0036] Table 1 Process parameters for preparing solid acid catalysts in Examples 1 to 5

[0037] The specific surface area and pore size of the solid acid catalysts obtained in Examples 1 to 5 and Comparative Examples 2 and 3 were measured using a specific surface area tester and a pore size analyzer BSD-660S, respectively. The specific test data are shown in Table 2.

[0038] Table 2 Specific surface area and pore size data of the obtained solid acid catalyst

[0039] From the data in Table 2, it can be seen that the specific surface areas of iron oxide and iron oxide / silicon oxide carriers are similar. After adding antimony trioxide, the specific surface area is greatly increased. However, with the change in the ratio of the three oxides, the specific surface area first increases and then decreases. The pore size and specific surface area have the same change pattern. It can be seen from the above performance indicators that the specific surface area and pore size data of the solid acid catalyst obtained in Example 3 are the best.

[0040] The lactose solutions obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were tested according to the liquid chromatography method in the 2015 Chinese Pharmacopoeia: Amino-bonded silica gel was used as filler, acetonitrile-water (70:30) was used as mobile phase, column temperature was 45°C, 10ul solution was passed through the column at a flow rate of 1.0ml / min, and the lactose content was tested at a wavelength of 238nm; the residual lactose content in each group of reaction solutions was tested: Catalytic rate = (original lactose amount - remaining lactose amount) / original lactose amount * 100%; The specific data are shown in Table 3.

[0041] Table 3 Lactose catalytic efficiency of the catalysts prepared in Examples 1 to 5 and Comparative Examples 1 to 3 for the first use

[0042] Combined with the data in Table 3, it can be seen that the SiO prepared by the present invention 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The catalytic efficiency of the solid acid catalyst is better than that of the liquid acid catalyst and can completely replace the liquid acid catalyst. 2 O 3 The content is the highest, the loaded sulfate ion is the largest, and the specific surface area of ​​Example 2 and Example 3 is larger. The above comprehensive data show that the catalytic efficiency of Example 1, Example 2 and Example 3 is similar, and the catalytic efficiency of Example 2 is the highest, reaching 87%.

[0043] Further testing of the SiO prepared by the present invention 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The service life test of the solid acid catalyst in the preparation of galactose is as follows: After each lactose catalysis, the solid acid catalysts of Comparative Examples 2, 3 and Examples 1 to 5 were filtered, activated, and used again for lactose catalysis. The lactose catalysis steps were the same, and the catalytic efficiency was recorded each time. The specific catalytic efficiency is shown in Table 4; wherein SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The activation method of the solid acid catalyst comprises the following steps: S11, adding the filtered and recovered solid acid catalyst into 68% sulfuric acid and shaking at 60° C. for 60 min; S12, Filtration of SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 Solid acid; S13, calcined at 300℃ to obtain SiO2 that can be added to lactose 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 Solid acid catalyst.

[0044] Table 4 Service life of solid acid catalysts used in Examples 1 to 5 and Comparative Examples 2 and 3

[0045] Comparing Comparative Example 2 with Comparative Example 3, silicon oxide helps to improve the stability of the structural skeleton and can extend the service life of the carrier; further comparing the comparative example with Examples 1 and 5, with the increase of silicon oxide, the skeleton structure is stable and the catalytic efficiency decays slowly.

[0046] From the above data, it can be seen that the SiO2 catalyst for catalyzing the conversion of lactose into galactose proposed in the present invention 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 The preparation method of solid acid catalyst comprises the following steps: firstly 2 O 3 Dissolves in sulfuric acid to form Fe 2 (SO 4 ) 3 solution, and then under heating conditions, Fe 2 (SO 4 ) 3 Reacts with water to form Fe 2 O 3 , the generated Fe 2 O 3 With SiO 2 Mixing, sulfuric acid with Fe 2 O 3 With SiO 2 Formation of SiO by solid-state reaction 2 / Fe 2 O 3 -SO 3 Solid acid; then to SiO 2 / Fe 2 O 3 -SO 3 Solid acid added to solid Sb 2 O 3 , rotating and stirring, heating until the mixture is molten, Fe 2 O 3 、SiO 2 and Sb 2 O 3 The outermost electrons of the three oxides intersect to obtain SiO 2 / Sb 2 O 3 / Fe 2 O 3 -SO 3 Solid acid; the solid acid catalyst obtained by the present invention is SiO 2 / Sb 2 O3 / Fe 2 O 3 As carrier, Fe 2 O 3 It is used to coordinate and adsorb sulfate. Silicon has a cross-linking effect. Iron, silicon and oxygen form a cross-linked structure, thereby stabilizing the structure and improving the dispersion of iron oxide. Antimony has a large molecular radius, and Sb is mixed into the carrier. 2 O 3 , a carrier with large porosity is obtained, which is more conducive to loading acid radicals. Therefore, the solid acid catalyst obtained by the present invention has a stable structure and strong acidity, and is applied to the production of galactose using lactose as a raw material. The superacid properties of the solid acid catalyst are fully utilized, and the porous structure and large specific surface area of ​​the obtained solid acid catalyst are combined to effectively increase the solid-liquid contact area. Therefore, the conversion efficiency is significantly improved, the separation rate is significantly improved, and it is convenient to recover and reuse.

Claims

1. A method for preparing a solid acid catalyst, characterized in that: The following steps are involved: S1, dissolving Fe2O3 in sulfuric acid to form Fe2(SO4)3 solution; S2, adding solid SiO2 to the ferric sulfate solution obtained in step S1, and heating the solid SiO2 and Fe2(SO4)3 solution under rotating stirring; During the heating process, Fe2(SO4)3 reacts with water to produce Fe2O3 and sulfuric acid; Under constant temperature conditions, the generated Fe2O3 is mixed with SiO2, and sulfuric acid and Fe2O3 / SiO2 form Fe2O3 / SiO2-SO3 solid acid; S3, adding solid Sb2O3 to the SiO2 / Fe2O3-SO3 solid acid obtained in step S2, rotating and stirring, and heating until the mixture is in a molten state, and Fe2O3, SiO2 and Sb2O3 are mutually melted to obtain SiO2 / Sb2O3 / Fe2O3-SO3 solid acid; S4, calcining to obtain the target solid acid catalyst.

2. The preparation method according to claim 1, characterized in that: The molar ratio of Fe2O3 to sulfuric acid in S1 is 1:(3.5~3.8).

3. The preparation method according to claim 1, characterized in that: The molar ratio of Fe2O3 to SiO2 in S2 is 1:(0.3~0.5).

4. The preparation method according to claim 1, characterized in that: In step S2, the constant temperature is 337° C. and the heating rate is 5° C. / min to 10° C. / min.

5. The preparation method according to claim 1, characterized in that: In step S3, the insulation temperature for the mutual melting of Fe2O3, SiO2 and Sb2O3 is 700°C, the heating rate is 5°C / min to 10°C / min, and nitrogen protection is used.

6. The preparation method according to claim 1, characterized in that: The molar ratio of Fe2O3 to Sb2O3 in step S3 is 1:(0.1~0.3).

7. The preparation method according to claim 1, characterized in that: The SiO2 / Sb2O3 / Fe2O3-SO3 solid acid obtained in step S3 is immersed in sulfuric acid, stirred and immersed at low temperature, and filtered to obtain a solid acid supplemented with sulfate ions.

8. A method for preparing galactose using the solid acid catalyst prepared by the preparation method according to any one of claims 1 to 7, characterized in that: Lactose and the solid acid catalyst are added into a reaction container for reaction; after the reaction is completed, the solid acid catalyst is filtered to obtain a galactose conversion liquid.

9. The method for preparing galactose according to claim 8, characterized in that : The activation method of SiO2 / Sb2O3 / Fe2O3-SO3 solid acid catalyst comprises the following steps: S11, adding the filtered and recovered solid acid catalyst into 68% sulfuric acid, soaking at low temperature, and shaking; S12, filtering SiO2 / Sb2O3 / Fe2O3-SO3 solid acid; S13, calcining to obtain SiO2 / Sb2O3 / Fe2O3-SO3 solid acid catalyst for lactose preparation.

Citation Information

Patent Citations

  • Sulfate radical composite oxide solid acid catalyst, its preparation method, and method for catalyzing conversion of xylan to furfural through using it

    CN103990473A

  • Method for catalytically decomposing wood fiber raw material

    CN109942835A

  • Porous magnetic carbon-based solid acid catalyst as well as preparation method and application thereof

    CN113578347A

  • Method for removing micro aldehyde group from 1,3-propylene glycol

    CN1803744A

  • Solid catalysts and method for preparing sugars using the same

    US20170166985A1