G-C3N4 / MXene composite photocatalytic material as well as preparation method and application thereof

By combining urea with MXene, the g-C3N4/MXene composite photocatalytic material formed by combining urea with MXene, the problem of insufficient absorption capacity of g-C3N4 for visible light is solved, the efficiency and antibacterial properties of the photocatalytic material are improved, and more efficient photocatalytic and Purification effect.

CN118925776APending Publication Date: 2024-11-12RES CENT FOR ECO ENVIRONMENTAL SCI THE CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410991117.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

g-C3N4 photocatalytic material has weak absorption capacity of visible light, resulting in low photocatalytic activity and efficiency in practical applications. The electronic structure and energy band structure lead to low separation efficiency of photogenerated charges, which reduces the efficiency of photocatalytic reactions .

Method used

Urea is used as the precursor of g-C3N4 and composited with MXene to form g-C3N4/MXene composite photocatalytic material through thermal polymerization process. The high conductivity and excellent light absorption performance of MXene are used to improve the visible light and near-infrared light absorption of photocatalytic materials. Ability to enhance the separation and transfer efficiency of photogenerated charges.

Benefits of technology

The photocatalytic degradation efficiency and antibacterial properties of photocatalytic materials are improved, and solar energy can be used more effectively and have a stronger purification effect during water treatment and antibacterial processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925776A_ABST
    Figure CN118925776A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of photocatalysis, in particular to a g-C3N4 / MXene composite photocatalytic material as well as a preparation method and application thereof. The preparation method comprises the following steps: taking urea as a precursor of g-C3N4, and compounding with MXene in a thermal polymerization process to form the g-C3N4 / MXene composite photocatalytic material. The preparation method is simple, mild in reaction condition and free of environmental pollution. The prepared g-C3N4 / MXene composite photocatalytic material has the advantages of high catalytic degradation efficiency and good antibacterial effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photocatalytic technology, and in particular to a g-C3N4 / MXene composite photocatalytic material and a preparation method and application thereof. Background Art

[0002] Photocatalytic technology has attracted widespread attention due to its high efficiency and environmental friendliness in the field of environmental purification and energy conversion. The core of this technology lies in photocatalysts, a material that can absorb light energy under light and generate bandgap excited state electrons, thereby promoting a series of chemical reactions such as oxidation, reduction and degradation.

[0003] g-C3N4 is a common photocatalytic material, which has been widely used in many fields such as environmental purification and energy conversion due to its wide light absorption range, low cost, high controllability and good photocatalytic activity. This material can effectively absorb ultraviolet rays in sunlight, and then excite electrons from the valence band to the conduction band, generating electron-hole pairs, which participate in redox reactions and degrade pollutants.

[0004] However, g-C3N4 also has some limitations in practical applications. The main problem is its relatively weak absorption capacity for visible light. The proportion of visible light in sunlight is as high as 45%. If this part of the spectrum can be fully utilized, the energy efficiency of photocatalysts will be greatly improved. In addition, the electronic structure and band structure of g-C3N4 lead to low separation efficiency of its photogenerated charges, which will cause electrons and holes to recombine before reaching the active sites of the reaction, thereby reducing the photocatalytic activity and efficiency. Summary of the invention

[0005] In order to solve or partially solve the problems existing in the related art, the present invention provides a g-C3N4 / MXene composite photocatalytic material and a preparation method and application thereof.

[0006] The present invention provides a method for preparing a g-C3N4 / MXene composite photocatalytic material, which comprises:

[0007] Urea is used as the precursor of g-C3N4 and is compounded with MXene during the thermal polymerization process to form a g-C3N4 / MXene composite photocatalytic material.

[0008] Further, the following steps are included:

[0009] a) slowly dripping the MXene few-layer dispersion into an ultrapure aqueous solution of urea and ultrasonically dissolving it to obtain a reaction stock solution;

[0010] b), drying and grinding the reaction stock solution to obtain a powdered raw material;

[0011] c) Under the protection of an inert gas, the powder raw material is calcined, and after calcination, it is cooled and ground to obtain a g-C3N4 / MXene composite photocatalytic material.

[0012] Furthermore, in step b), the drying temperature is 55-65° C. and the drying time is 12-48 hours.

[0013] Furthermore, the mass ratio of urea to MXene in the reaction stock solution is 1000:(1.0-3.5).

[0014] Furthermore, the ultrasound in step a) is ice bath ultrasound, and the ultrasound time is 1 to 3 hours.

[0015] Furthermore, the inert gas is nitrogen.

[0016] Furthermore, in the step c), the calcination temperature is 500-600° C., the calcination time is 1-3 hours, and the heating rate is 8-12° C. / min.

[0017] The present invention also provides a g-C3N4 / MXene composite photocatalytic material, which is prepared according to any of the methods described above.

[0018] The present invention also provides an application of the g-C3N4 / MXene composite photocatalytic material in the fields of water treatment and antibacterial.

[0019] Furthermore, during the water treatment and / or antibacterial treatment process, the g-C3N4 / MXene composite photocatalytic material is compounded with persulfate for use.

[0020] The g-C3N4 / MXene composite photocatalytic material provided by the present invention and its preparation method and application include the following beneficial effects:

[0021] The preparation method prepares a mixed solution of urea and MXene in advance, and then after drying and grinding, the obtained powder raw material is calcined under the protection of inert gas. During the thermal decomposition and polymerization of urea, g-C3N4 and MXene are composited to form a photocatalytic material. The preparation method is simple, the reaction conditions are mild, and it is environmentally friendly.

[0022] The prepared g-C3N4 / MXene composite photocatalytic material MXene has excellent light absorption properties and can absorb light in the visible light and even near-infrared light region, which helps to broaden the light response range of g-C3N4 and improve the utilization efficiency of solar energy. The high conductivity of MXene helps the rapid transmission of photogenerated electrons and reduces the recombination of electrons and holes, thereby improving the charge separation efficiency in the photocatalytic process. Therefore, the photogenerated charge separation and transfer of the composite photocatalytic material are more efficient, improving the photocatalytic degradation efficiency. In addition, in water treatment, the g-C3N4 / MXene composite photocatalytic material exhibits stronger antibacterial properties, which helps to more effectively inactivate microorganisms during disinfection and purification.

[0023] In summary, the g-C3N4 / MXene composite photocatalytic material prepared by the present invention has the advantages of high catalytic degradation efficiency and good antibacterial effect.

[0024] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The above and other objects, features and advantages of the early warning unit of the present invention will become more apparent by describing in more detail exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like parts in the exemplary embodiments of the present invention.

[0026] Figure 1 is a scanning electron microscope image of the g-C3N4 / MXene composite photocatalytic material prepared in Example 1 of the present invention;

[0027] Figure 2 is a scanning electron microscope image of the g-C3N4 photocatalytic material prepared in Comparative Example 1 of the present invention;

[0028] Figure 3 is a scanning electron microscope image of MXene used in the embodiments of the present invention;

[0029] Figure 4 is a kinetic model curve of phenol degradation by photocatalysis in an embodiment of the present invention;

[0030] Figure 5 This is a diagram showing the effect of g-C3N4 / MXene activated persulfate composite system on the degradation of phenol in an embodiment of the present invention;

[0031] Figure 6 This is a diagram showing the effect of g-C3N4 / MXene activated persulfate composite system on the degradation of phenol in an embodiment of the present invention;

[0032] Figure 7This is a diagram showing the effect of photocatalyst activation of a persulfate composite system for degrading phenol in an embodiment of the present invention;

[0033] Figure 8 This is a diagram showing the effect of photocatalyst activation of a persulfate composite system for degrading phenol in an embodiment of the present invention;

[0034] Fig. 9 This is a diagram showing the effect of g-C3N4 / MXene activated persulfate composite system on the degradation of phenol in an embodiment of the present invention;

[0035] Fig.10 is a bar graph of the sterilization rate of Escherichia coli by the photocatalyst activated persulfate composite system in the embodiment of the present invention;

[0036] Fig.11 This is a diagram showing the antibacterial effect of the photocatalyst activated persulfate composite system on Escherichia coli in an embodiment of the present invention;

[0037] Fig.12 is a bar graph of the sterilization rate of Staphylococcus aureus by the photocatalyst activated persulfate composite system in the embodiment of the present invention;

[0038] Fig.13 1 is a diagram showing the antibacterial effect of the photocatalyst activated persulfate composite system on Staphylococcus aureus in an embodiment of the present invention. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The singular forms "a", "the" and "the" used in the present invention and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0041] It should be understood that although the terms "first", "second", "third", etc. may be used to describe various information in the present invention, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0042] MXene is a type of two-dimensional material with high conductivity, which is obtained by chemical exfoliation of metal silicates (MAX phase). It has excellent conductivity, low resistance and high electron mobility, which is conducive to the transmission of electrons and the separation of photogenerated charges. MXene materials have good light absorption performance in the visible and near-infrared spectrum. It can absorb most of the visible light and part of the infrared light, so that MXene can effectively utilize light energy in a wide range of spectra. MXene materials show excellent photocatalytic activity, which can excite electrons and produce active oxygen species (such as ·OH and ·O2 - ). Its high conductivity and large specific surface area are helpful for the separation of photogenerated charges and the exposure of catalytic active centers, thus improving the efficiency of photocatalytic reaction. Therefore, the inventors of the present application considered compounding MXene with g-C3N4 to improve the photocatalytic activity and efficiency of g-C3N4.

[0043] The present invention provides a method for preparing a g-C3N4 / MXene composite photocatalytic material, which comprises:

[0044] Urea is used as the precursor of g-C3N4 and is compounded with MXene during the thermal polymerization process to form a g-C3N4 / MXene composite photocatalytic material.

[0045] In the preparation method provided in this embodiment, MXene is compounded on g-C3N4 while synthesizing g-C3N4 by thermal polymerization. The effect of thermal polymerization and compounding at the same time is:

[0046] Moreover, the inventors of the present application have found through research that MXene is selective for g-C3N4 precursors, which is manifested in that the photocatalytic performance of the g-C3N4 / MXene composite materials obtained by using different organic compounds containing carbon and nitrogen (such as urea, melamine, dicyandiamide, etc.) as precursors is quite different. The inventors of the present application have further found that using urea as a precursor is conducive to obtaining a composite photocatalytic material with better photocatalytic performance.

[0047] The above preparation method may specifically include the following steps:

[0048] a) slowly dripping the MXene few-layer dispersion into an ultrapure aqueous solution of urea and ultrasonically dissolving it to obtain a reaction stock solution;

[0049] b), drying and grinding the reaction stock solution to obtain a powdered raw material;

[0050] c) Under the protection of an inert gas, the powder raw material is calcined, and after calcination, it is cooled and ground to obtain a g-C3N4 / MXene composite photocatalytic material.

[0051] a) Mixing MXene few-layer dispersion and urea solution:

[0052] The above step a) is used to evenly disperse MXene in the urea solution, laying the foundation for the subsequent thermal polymerization reaction and composite material formation. This step adopts ultrasonic treatment, which helps to further peel and disperse MXene, prevent the restacking of materials, ensure uniform mixing with the urea solution, and thus ensure the uniformity of the combination of MXene and g-C3N4 in the subsequent thermal polymerization. In order to prevent MXene from oxidizing during the ultrasonic process, the ultrasound in this step is preferably ice bath ultrasound. The ultrasonic time is preferably 1 to 3 hours, and most preferably 2 hours.

[0053] This step may specifically include:

[0054] a1), dissolving urea in ultrapure water, stirring and ultrasonically mixing to obtain a urea solution;

[0055] a2) Slowly drop the MXene few-layer dispersion into the urea solution and ultrasonicate it in an ice bath to obtain the reaction stock solution.

[0056] After step a), a reaction stock solution in which g-C3N4 and MXene are evenly dispersed can be obtained. The mass ratio of urea to MXene in the reaction stock solution is preferably 1000:(1.0-3.5), specifically 1000:1.0, 1000:1.5, 1000:2.0, 1000:2.5, 1000:3.0, 1000:3.5, and the most preferred ratio in this embodiment is 1000:1.5. The concentration of MXene in the added MXene few-layer dispersion is preferably 3-6 mg / mL, more preferably 5 mg / mL.

[0057] The above step b) is a step of drying and grinding the reaction stock solution. Drying is used to remove moisture so that urea and MXene form a solid mixture. Grinding is to increase the specific surface area of ​​the powder, which helps to improve the reactivity of the material and the subsequent calcination efficiency. Drying can be carried out in a blast drying oven. The drying temperature is preferably 55 to 65°C, specifically 55°C, 57°C, 59°C, 60°C, 61°C, 62°C, 65°C, etc., and of course other values ​​within the above range. The drying temperature is most preferably 60°C. The inventors of the present application have found that the drying time is important for the performance of the final product. For this reason, the present application controls the drying time to be 12 to 48h, specifically 12h, 24, 36h, 40h, 48h, etc., and of course other values ​​within the above range. The drying time is most preferably 36h.

[0058] The above step c) is a step of calcining the powdered raw material under the protection of an inert gas. Calcination is a step in preparing the formation of a g-C3N4 / MXene composite material. The calcination process not only promotes the thermal decomposition and polymerization of urea, but also helps to form a composite structure between g-C3N4 and MXene. Inert gas protection can prevent the material from oxidizing at high temperatures, maintaining the conductivity of MXene and the structural integrity of g-C3N4. The inventors of the present application have found through research that the choice of inert gas has an impact on the performance of the final product. Compared with argon, the photocatalytic performance of the composite photocatalytic material obtained in a nitrogen calcination environment is better, so in this embodiment, the inert gas is preferably nitrogen.

[0059] In step c), the calcination temperature is preferably 500-600°C, specifically 500°C, 520°C, 530°C, 550°C, 560°C, 580°C, 600°C, etc., and of course other values ​​within the above range can also be used. The calcination time is preferably 1-3h, specifically 1h, 1.5h, 2h, 2.0h, 2.5h, 3.0h, etc., and of course other values ​​within the above range can also be used. The heating rate is preferably 8-12°C / min, specifically 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, etc. The most preferred calcination conditions are as follows: the calcination temperature is 550°C, the calcination time is 2h, and the heating rate is 10°C / min.

[0060] The calcined material can be cooled and ground to obtain the g-C3N4 / MXene composite photocatalytic material.

[0061] Another embodiment of the present invention also provides a g-C3N4 / MXene composite photocatalytic material, which is prepared according to the method of the above embodiment. The specific implementation is the same as the above embodiment and is not repeated here. In the composite photocatalytic material, g-C3N4 and MXene cooperate with each other, not only showing high photocatalytic performance, but also showing strong antibacterial effect, so it can be used for the treatment of pollutants in water (such as phenol), or antibacterial treatment (such as Escherichia coli, Staphylococcus aureus).

[0062] The preparation method of the g-C3N4 / MXene composite photocatalytic material provided in this embodiment has the following advantages:

[0063] The method prepares a mixed solution of urea and MXene in advance, and then after drying and grinding, the obtained powder raw material is calcined under the protection of inert gas. During the thermal decomposition and polymerization of urea, g-C3N4 and MXene are composited to form a photocatalytic material. The preparation method is simple, the reaction conditions are mild, and it is environmentally friendly.

[0064] The prepared g-C3N4 / MXene composite photocatalytic material has the following advantages:

[0065] MXene has excellent light absorption properties and can absorb light in the visible and even near-infrared regions, which helps to broaden the light response range of g-C3N4 and improve the efficiency of solar energy utilization. The high conductivity of MXene helps the rapid transmission of photogenerated electrons, reduces the recombination of electrons and holes, and thus improves the charge separation efficiency in the photocatalytic process. Therefore, the separation and transfer of photogenerated charges in the composite photocatalytic material are more efficient, improving the efficiency of photocatalytic degradation.

[0066] In addition, in water treatment, g-C3N4 / MXene composite photocatalytic materials exhibit enhanced antibacterial properties, which helps to more effectively inactivate microorganisms during disinfection and purification processes.

[0067] In summary, the g-C3N4 / MXene composite photocatalytic material has the advantages of high catalytic degradation efficiency and good antibacterial effect.

[0068] Another embodiment of the present invention also provides an application of the above-mentioned g-C3N4 / MXene composite photocatalytic material in the fields of water treatment and antibacterial.

[0069] The application method may specifically be:

[0070] The g-C3N4 / MXene composite photocatalytic material is uniformly dispersed in the wastewater sample or bacterial sample to be treated to form a stable suspension;

[0071] The suspension was illuminated using a xenon lamp equipped with a 400 nm filter as the light source.

[0072] A xenon lamp with a 400nm filter provides light to excite the photocatalyst g-C3N4 / MXene to produce photocatalytic activity. Ultraviolet light or visible light is used as a light source to excite g-C3N4 to produce electron-hole pairs, which participate in redox reactions to degrade organic pollutants in water or inactivate microorganisms.

[0073] After light treatment, separation and recovery can also be carried out: the photocatalyst can be separated from the water sample by filtration, sedimentation or centrifugation for recovery and reuse.

[0074] During the water treatment and / or antibacterial treatment, the g-C3N4 / MXene composite photocatalytic material can be used in combination with persulfate. That is, the g-C3N4 / MXene composite photocatalytic material and persulfate are uniformly dispersed in the wastewater sample or bacterial sample to be treated to form a stable suspension; and then the above-mentioned light treatment is performed. The above-mentioned persulfate is preferably potassium persulfate.

[0075] The g-C3N4 / MXene composite photocatalytic material is used in combination with persulfate, and the strong oxidizing ability of persulfate is utilized to generate highly active free radicals through activation, thereby improving the degradation efficiency of pollutants such as phenol in water, and the ability to kill microorganisms such as Escherichia coli in water. This combination provides an efficient water treatment technology that helps to achieve rapid degradation of pollutants and inactivation of microorganisms in a shorter period of time.

[0076] The technical solution of the present invention is further described below in conjunction with specific embodiments:

[0077] The MXene few-layer dispersions in the following examples were purchased from Xianfeng Nanotechnology Co., Ltd., model number NO: XFK11, concentration 5 mg / mL. Figure 3 shown.

[0078] Example 1

[0079] (1) Take 5 g of urea and put it in a 50 ml centrifuge tube. Add 20 ml of ultrapure water and sonicate it at 50 W for 30 min to obtain a fully dissolved urea solution.

[0080] (2) Slowly add 1.5 ml of MXene few-layer dispersion to the urea solution, and then ultrasonicate at 50 W in an ice-water bath for 120 min to obtain the reaction stock solution (the mass ratio of urea to MXene is 1000:1.5).

[0081] (3) The reaction stock solution was placed in a forced air drying oven at 60° C. and dried for 36 h, and then ground into powder to obtain a powder raw material.

[0082] (4) The powder raw material was placed in a quartz boat and calcined at 550°C for 2 hours in a tube furnace with high-purity argon gas. The heating rate was 10°C / min. After the tube furnace was cooled to room temperature, the solid was ground to obtain a g-C3N4 / MXene composite photocatalytic material. The scanning electron microscope image is shown below: Figure 1 shown.

[0083] Embodiment 2 to Embodiment 4

[0084] The only difference from Example 1 is that the drying temperatures in step (3) are 12 h, 24 h and 40 h respectively.

[0085] Embodiment 5-embodiment 6

[0086] The only difference from Example 1 is that the amounts of MXene few-layer dispersion added in step (2) are 2.5 ml (the mass ratio of urea to MXene is 1000:2.5) and 3.5 ml (the mass ratio of urea to MXene is 1000:3.5), respectively.

[0087] Comparative Example 1

[0088] (1) Take 5 g of urea and put it in a 50 ml centrifuge tube. Add 20 ml of ultrapure water and sonicate it at 50 W for 30 min to obtain a fully dissolved urea solution.

[0089] (3) The urea solution was placed in a forced air drying oven and dried at 60° C. for 36 h, and then ground into powder to obtain urea powder.

[0090] (4) Put the urea powder into a quartz boat and calcine it at 550℃ for 2h in a tube furnace with high-purity argon gas. The heating rate is 10℃ / min. After the tube furnace is cooled to room temperature, grind the solid to obtain g-C3N4 photocatalytic material. The scanning electron microscope image is as follows: Figure 2 shown.

[0091] Depend on Figure 1 , Figure 2 and Figure 3 It can be seen that the g-C3N4 / MXene composite photocatalytic material was successfully prepared.

[0092]

Phenol degradation kinetic model

[0093] Analyzed objects:

[0094] Experimental group A: g-C3N4 / MXene composite photocatalytic material prepared in Example 1

[0095] Experimental group B: g-C3N4 / MXene composite photocatalytic material prepared in Example 1 + potassium persulfate

[0096] Control group A': g-C3N4 photocatalyst prepared in Comparative Example 1

[0097] Control group B': g-C3N4 photocatalyst prepared in Comparative Example 1 + potassium persulfate

[0098] Analytical methods:

[0099] Example A and Comparative Example A':

[0100] Take 3 mg of catalyst powder and add it to 30 ml of 10 mg / L phenol solution. Mix it evenly by ultrasonic and place it under a 300 W xenon lamp (400 nm filter) for photocatalytic reaction. Sampling is performed every five minutes. After sampling, the sample is filtered through a 0.22 μm water filter membrane. The filtered sample is analyzed by liquid chromatography. The phenol degradation kinetic model curve is fitted as shown in the figure: Figure 4 shown.

[0101] Example B and Comparative Example B':

[0102] Take 3 mg of catalyst powder and add it to 30 ml of 10 mg / L phenol solution (containing 5 mM potassium persulfate), mix it evenly with ultrasound and put it under a 300 W xenon lamp (light intensity: 150 mW / cm 2 The photocatalytic reaction was carried out under a 400 nm filter, and samples were taken every five minutes. After sampling, the samples were filtered through a 0.22 μm water filter membrane, and the filtered samples were analyzed by liquid chromatography. The phenol degradation kinetic model curve was fitted as shown in FIG. Figure 4 shown.

[0103] Depend on Figure 4 It can be seen that the degradation effect of experimental group B is the best, and the degradation efficiency is nearly 5 times that of the control group B'. The degradation efficiency of experimental group A is 5.5 times that of the control group A', indicating that the photocatalytic performance of g-C3N4 / MXene composite photocatalytic material is good.

[0104] [Effect of drying time on product performance]

[0105] Analyzed objects:

[0106] Experimental group 36h: g-C3N4 / MXene composite photocatalytic material prepared in Example 1 + potassium persulfate Experimental group 12h: g-C3N4 / MXene composite photocatalytic material prepared in Example 2 + potassium persulfate Experimental group 24h: g-C3N4 / MXene composite photocatalytic material prepared in Example 3 + potassium persulfate Experimental group 40h: g-C3N4 / MXene composite photocatalytic material prepared in Example 4 + potassium persulfate Analysis method:

[0107] Take 3 mg of catalyst powder and add it to 30 ml of 10 mg / L phenol solution (containing 5 mM potassium persulfate), mix it evenly with ultrasound and put it under a 300 W xenon lamp (light intensity: 150 mW / cm 2The photocatalytic reaction was carried out under a 400nm filter, and samples were taken every ten minutes. After sampling, the samples were filtered through a 0.22-micron water filter membrane, and the filtered samples were analyzed by liquid chromatography. The effect of the g-C3N4 / MXene activated persulfate composite system on the degradation of phenol is shown in the figure below. Figure 5 shown.

[0108] Depend on Figure 5 It can be seen that the drying time has an impact on the performance of the photocatalyst product, and the degradation effect of the photocatalyst product with a drying time of 36h is the best.

[0109] [The influence of raw material ratio on product performance]

[0110] Experimental group 1.5‰: g-C3N4 / MXene composite photocatalytic material prepared in Example 1 + potassium persulfate Experimental group 2.5‰: g-C3N4 / MXene composite photocatalytic material prepared in Example 5 + potassium persulfate Experimental group 3.5‰: g-C3N4 / MXene composite photocatalytic material prepared in Example 6 + potassium persulfate Analysis method:

[0111] Take 3 mg of catalyst powder and add it to 30 ml of 10 mg / L phenol solution (containing 5 mM potassium persulfate), mix it evenly with ultrasound and put it under a 300 W xenon lamp (light intensity: 150 mW / cm 2 The photocatalytic reaction was carried out under a 400nm filter, and samples were taken every ten minutes. After sampling, the samples were filtered through a 0.22-micron water filter membrane, and the filtered samples were analyzed by liquid chromatography. The effect of the g-C3N4 / MXene activated persulfate composite system on the degradation of phenol is shown in the figure below. Figure 6 shown.

[0112] [The influence of raw materials on product performance]

[0113] Comparative Example 2

[0114] The only difference from Example 1 is that urea is replaced by melamine. The rest is the same as Example 1.

[0115] Comparative Example 3

[0116] The difference from Comparative Example 1 is that urea is replaced by melamine. The rest is the same as Comparative Example 1.

[0117] Analyzed objects:

[0118] Experimental group B: g-C3N4 / MXene composite photocatalytic material prepared in Example 1 + potassium persulfate

[0119] Control group B': g-C3N4 photocatalyst prepared in Comparative Example 1 + potassium persulfate

[0120] Control group C: g-C3N4 / MXene composite photocatalytic material prepared in comparative example 2 + potassium persulfate

[0121] Control group D: g-C3N4 photocatalyst prepared in Comparative Example 3 + potassium persulfate

[0122] Analytical methods:

[0123] Take 3 mg of catalyst powder and add it to 30 ml of 10 mg / L phenol solution (containing 5 mM potassium persulfate), mix it evenly with ultrasound and put it under a 300 W xenon lamp (light intensity: 150 mW / cm 2 The photocatalytic reaction was carried out under a 400nm filter, and samples were taken every ten minutes. After sampling, the samples were filtered through a 0.22 micron water filter membrane, and the filtered samples were analyzed by liquid chromatography. The effect of the photocatalyst activated persulfate composite system on the degradation of phenol is shown in the figure below. Figure 7 shown.

[0124] Depend on Figure 7 It can be seen that the choice of g-C3N4 precursor has an impact on product performance, and the product made with urea as the precursor has better performance.

[0125] [The impact of inert gas environment on product performance]

[0126] Example 7

[0127] The only difference from Example 1 is that in step (4), nitrogen is replaced by argon. The rest is the same as Example 1.

[0128] Comparative Example 4

[0129] The only difference from Comparative Example 1 is that in step (4), nitrogen is replaced by argon. The rest is the same as Comparative Example 1.

[0130] Analyzed objects:

[0131] Experimental group N2-MCN: g-C3N4 / MXene composite photocatalytic material prepared in Example 1 + potassium persulfate

[0132] Experimental group Ar2-MCN: g-C3N4 / MXene composite photocatalyst prepared in Example 7 + persulfate Control group N2-CN: g-C3N4 photocatalyst prepared in Comparative Example 1 + potassium persulfate

[0133] Control group Ar2-CN: g-C3N4 photocatalyst prepared in Comparative Example 4 + potassium persulfate

[0134] Analytical methods:

[0135] Take 3 mg of catalyst powder and add it to 30 ml of 10 mg / L phenol solution (containing 5 mM potassium persulfate), mix it evenly with ultrasound and put it under a 300 W xenon lamp (light intensity: 150 mW / cm 2 The photocatalytic reaction was carried out under a 400nm filter, and samples were taken every ten minutes. After sampling, the samples were filtered through a 0.22 micron water filter membrane, and the filtered samples were analyzed by liquid chromatography. The effect of the photocatalyst activated persulfate composite system on the degradation of phenol is shown in the figure below. Figure 8 shown.

[0136] Depend on Figure 8 It can be seen that the choice of inert gas in the calcination environment has an impact on product performance, and the degradation effect of the product with nitrogen as the inert gas is better than that of the product with argon as the inert gas.

[0137] [Effect of potassium persulfate concentration on degradation effect]

[0138] Analyzed objects:

[0139] Experimental group 3mM PMS: phenol solution (containing 3mM potassium persulfate)

[0140] Experimental group 5mM PMS: phenol solution (containing 5mM potassium persulfate)

[0141] Experimental group 10mM PMS: phenol solution (containing 10mM potassium persulfate)

[0142] Experimental group 15mM PMS: phenol solution (containing 15mM potassium persulfate)

[0143] Analytical methods:

[0144] Take 3 mg of the catalyst powder prepared in Example 1 and add it to 30 ml of 10 mg / L phenol solution (containing potassium persulfate), mix it evenly with ultrasound and place it under a 300 W xenon lamp (light intensity: 150 mW / cm 2 The photocatalytic reaction was carried out under a 400nm filter, and samples were taken every five minutes. After sampling, the samples were filtered through a 0.22 micron water filter membrane, and the filtered samples were analyzed by liquid chromatography. The effect of the g-C3N4 / MXene activated persulfate composite system on the degradation of phenol is shown in the figure Fig. 9 shown.

[0145] Depend on Fig. 9 It can be seen that when PMS is used in combination with the g-C3N4 / MXene activated persulfate prepared in this application, the degradation effect is best when the addition amount is 5mM.

[0146]

Escherichia coli antibacterial test

[0147] Analyzed objects:

[0148] Experimental group MCN: g-C3N4 / MXene composite photocatalyst prepared in Example 1 + potassium persulfate Control group CN: g-C3N4 photocatalyst prepared in Comparative Example 1 + potassium persulfate

[0149] Blank control group PMS: potassium persulfate

[0150] Analytical methods:

[0151] (1) Take 4 mg of photocatalyst material (blank control group without photocatalyst material) and dissolve it in 18 ml of saline solution (containing 5 mM potassium persulfate) and disperse it evenly by ultrasonication.

[0152] (2) Add 2 ml OD 600 = 1.00 E. coli solution (the number of E. coli in the system is 10 8 CFU / ml) and mix well.

[0153] (3) Irradiate with visible light (300W xenon lamp intensity: 150mW / cm 2 , 400nm filter) and dilute the bacterial solution on LB solid culture medium and spread it on the plate at 5min intervals.

[0154] (4) Place the cells in a 30°C constant temperature incubator for 48 hours and observe the number of E. coli.

[0155] The bactericidal rate of photocatalyst against Escherichia coli is as follows Fig.10 The antibacterial effect on Escherichia coli is shown in the figure Fig.11 shown.

[0156] Depend on Fig.10 and Fig.11 It can be seen that the g-C3N4 / MXene composite photocatalytic material prepared in this example has a high antibacterial effect on Escherichia coli. 8 CFU / ml of Escherichia coli can be completely inactivated.

[0157]

Staphylococcus aureus antibacterial experiment

[0158]

Escherichia coli antibacterial test

[0159] Analyzed objects:

[0160] Experimental group MCN: g-C3N4 / MXene composite photocatalyst prepared in Example 1 + potassium persulfate Control group CN: g-C3N4 photocatalyst prepared in Comparative Example 1 + potassium persulfate

[0161] Blank control group PMS: potassium persulfate

[0162] Analytical methods:

[0163] (1) Take 4 mg of photocatalyst material (blank control group without photocatalyst material) and dissolve it in 19.8 ml of saline solution (containing 5 mM potassium persulfate) and disperse it evenly by ultrasonication.

[0164] (2) Add 0.2 ml OD 600 = 0.1 of Staphylococcus aureus solution (the number of Staphylococcus aureus in the system is 10 6 CFU / ml) and mix well.

[0165] (3) Irradiate with visible light (300W xenon lamp intensity: 150mW / cm 2 , 400 nm filter) and dilute the bacterial solution on LB solid medium and spread on the plate at 10 min intervals.

[0166] (4) Place the cells in a 30°C constant temperature incubator for 48 hours and observe the number of E. coli.

[0167] The bactericidal rate of photocatalyst against Staphylococcus aureus is as follows Fig.12 The antibacterial effect on Staphylococcus aureus is shown in Fig.13 shown.

[0168] Depend on Fig.12 and Fig.13 It can be seen that the g-C3N4 / MXene composite photocatalytic material prepared in this example has a high antibacterial effect on Staphylococcus aureus. 6 CFU / ml of Staphylococcus aureus can be completely inactivated.

[0169] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing a g-C3N4 / MXene composite photocatalytic material, characterized in that: include: Urea is used as the precursor of g-C3N4 and is compounded with MXene during the thermal polymerization process to form a g-C3N4 / MXene composite photocatalytic material.

2. The preparation method according to claim 1, characterized in that: The steps include: a) slowly dripping the MXene few-layer dispersion into an ultrapure aqueous solution of urea and ultrasonically dissolving it to obtain a reaction stock solution; b), drying and grinding the reaction stock solution to obtain a powdered raw material; c) Under the protection of an inert gas, the powder raw material is calcined, and after calcination, it is cooled and ground to obtain a g-C3N4 / MXene composite photocatalytic material.

3. The preparation method according to claim 1, characterized in that: In the step b), the drying temperature is 55-65° C. and the drying time is 12-48 hours.

4. The preparation method according to claim 1, characterized in that: The mass ratio of urea to MXene in the reaction stock solution is 1000:(1.0-3.5).

5. The preparation method according to claim 1, characterized in that: The ultrasound in step a) is performed by ice bath ultrasound, and the ultrasound time is 1 to 3 hours.

6. The preparation method according to claim 1, characterized in that: The inert gas is nitrogen.

7. The preparation method according to claim 1, characterized in that: In the step c), the calcination temperature is 500-600° C., the calcination time is 1-3 hours, and the heating rate is 8-12° C. / min.

8. A g-C3N4 / MXene composite photocatalytic material, characterized in that: It is prepared according to the method according to any one of claims 1 to 7.

9. Application of the g-C3N4 / MXene composite photocatalytic material according to claim 8 in the fields of water treatment and antibacterial.

10. The use according to claim 9, characterized in that: During water treatment and / or antibacterial treatment, the g-C3N4 / MXene composite photocatalytic material is compounded with persulfate for use.

Citation Information

Patent Citations

  • Preparation method of two-dimensional titanium carbide / two-dimensional graphite phase carbon nitride nanosheet heterojunction and application of heterojunction in photocatalytic reduction of CO2

    CN111215115A

  • Efficient photocatalyst, preparation method and application

    CN114653393A

  • O-g-C3N4 photocatalytic coupling persulfate, preparation method thereof and application of O-g-C3N4 photocatalytic coupling persulfate in degradation of resistant genes

    CN115301273A

  • Hydroxyl functionalized titanium carbide loaded carbon nitride photocatalyst as well as preparation and application thereof

    CN116196959A

  • Ti3C2 / g-C3N4 composite photocatalyst as well as preparation method and application thereof

    CN116571266A

Cited By

  • Catalytic ozonation water treatment method for regulating and controlling structural characteristics of MXene by carbon nitride

    CN120644227A