Acid-modified supported COFs catalyst as well as preparation method and application thereof
Through the acid-modified supported COFs catalyst in the alkylation reaction of nitrobenzene compounds, the regular pore structure and acidic functional groups of COFs materials are used to solve the problems of insufficient environmental pollution and catalytic performance in traditional processes, achieving high Conversion rate, high selectivity and stability, suitable for industrial applications.
Patent Information
- Application Number
- CN202410811265.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-12
AI Technical Summary
The use of liquid acid in the alkylation process of existing nitrobenzene compounds causes environmental pollution and device corrosion, insufficient catalyst conversion and selectivity, and irregular pore structure of traditional support, affecting catalytic performance.
Using acid-modified supported COFs catalyst, metal nanoparticles are loaded through the high specific surface area and regular pore structure of COFs material, combined with grafting method, the alkylation reaction of nitrobenzene compounds is realized, and the addition of the Acid reagents to improve catalytic performance and stability.
It improves the conversion, selectivity and stability of the catalyst, reduces process costs, conforms to the trend of green chemistry, and has a high dispersion of the loaded metal, avoids metal agglomeration, and is suitable for industrial applications.
Smart Images

Figure BDA0004906231900000051 
Figure BDA0004906231900000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of alkylanilinization of nitrobenzene compounds, and in particular to an acid-modified supported COFs catalyst and a preparation method and application thereof. Background Art
[0002] Alkylaniation of nitrobenzene compounds refers to the process of converting nitrobenzene compounds into the corresponding amino compounds (aniline), which are then further reacted with alkylating agents to form alkylated aniline. This process is usually divided into two steps.
[0003] 1) Nitro reduction: Nitrobenzene must first undergo a reduction reaction to reduce the nitro group to an amino group. 2) Alkylation of aniline: After aniline is formed, it can react with an alkylating agent in a variety of ways. At present, the production process is mainly divided into two methods, one is a two-step method, i.e., nitro reduction and alkylation react separately, and the other is a one-step reaction of nitro reduction and alkylation. Both require the use of metal powder and acid as a reduction system during the reaction. The one-step method is more widely used in the process flow due to its simple process and low process operation difficulty, but it is necessary to add liquid acid to the reaction to enhance the acid catalytic function. Due to the improvement of national standards in the new century and the trend of green chemistry, the addition of liquid acid produces greater pollution, so this step needs to be improved, among which replacing it with solid acid has become a new research direction.
[0004] Alkylaniline is a large class of compounds, among which pendimethalin of the dinitrotoluidine class is the largest herbicide and is widely used in agricultural production. There are two main routes for the synthesis of pendimethalin. Among them, the 3,4-dimethylnitrobenzene synthesis route has the characteristics of short synthesis route, low initial investment, high product yield, and low price of reaction substrate, so it is favored by investors in the chemical industry. N-(1-ethylpropyl)-3,4-dimethylaniline, as a precursor of pendimethalin, is more widely used in the industry, but the catalysts and acidic reagents required in the above-mentioned synthesis route have a great impact on the environment, high acid and alkali resistance requirements for equipment, and the reaction conversion rate and selectivity need to be further improved. Therefore, the development of new catalysts is imminent.
[0005] At present, conventional catalysts mainly use activated carbon as a carrier, and the carrier pore structure is irregular and normally distributed. And the overall reaction process requires the addition of liquid acid, which will inevitably cause environmental pollution and equipment corrosion. Therefore, companies need to increase investment in environmental protection. For example, patent CN113735717A reports the use of 37% waste nitric acid to prepare dimethoate, and 37% of the waste nitric acid can also be recycled. And patent CN109796347A reports a dimethoate production process without nitric acid wastewater discharge. However, these technical solutions have high requirements on production processes and costs. Therefore, regular pore structures and how to impart different catalytic functions to carriers have become goals that need to be solved.
[0006] COFs are connected by covalent bonds in terms of structural composition, so COFs materials are difficult to be destroyed by chemical reagents, are limited by high temperature and high pressure, and have strong chemical stability and thermal stability. Affected by the monomer, COFs materials have a highly ordered pore structure, and metal nanoparticles / active groups can be loaded / grafted inside and outside the pores to improve the selectivity and stability of the reaction. The regular pore structure is not only conducive to material transfer, but also improves the reaction rate and catalyst activity, and the metal (or other active centers) fixed in the COFs cavity has a high degree of dispersion. Therefore, under low metal loading and mild reaction conditions, the catalyst can show excellent catalytic performance. And the stability of the supported COFs catalyst is high, easy to recycle and reuse, and the catalyst activity can be maintained for a long time. Compared with other types of COFs, the COFs ligands in the present invention are low in cost and have price advantages.
[0007] In summary, new catalysts, especially those with COFs as carriers, have diversified catalyst design, multiple catalytic functions and price advantages. Compared with traditional catalysts, COFs are more flexible in external active groups and have higher dispersion in loaded metal particles, which can maximize metal utilization. In the application of nitrobenzene hydrogenation and N-alkylation reactions, this catalyst has bid farewell to the previous dilemma of environmental pollution and corrosion of reaction equipment, and has great value in industrial applications. Summary of the invention
[0008] In view of the problems existing in the above-mentioned prior art, the first purpose of the present invention is to solve the problem of agglomeration of metal particles on a carrier, and to provide a method for preparing an acid-modified supported COFs catalyst.
[0009] The second object of the present invention is to provide an acid-modified supported COFs catalyst.
[0010] The third object of the present invention is to provide an application of an acid-modified supported COFs catalyst in the alkylanilinization of nitrobenzene compounds, taking the synthesis of N-(1-ethylpropyl)-3,4-dimethylaniline as an example, to improve its conversion rate and selectivity.
[0011] To achieve the above object, the present invention adopts the following technical solution:
[0012] In a first aspect, the present invention provides a method for preparing an acid-modified supported COFs catalyst, which is carried out according to the following steps:
[0013] 1) Preparation of COFs: Pyridine compounds and aldehyde compounds are added to a reactor respectively, mixed evenly, and then a polymerization agent is added; the reactor is placed in liquid nitrogen for freezing, and then the reactor is sealed and evacuated until the pressure is displayed below 50 mTorr; then the temperature is raised to 120°C-200°C for reaction for 10-100 hours, and finally the reactor is opened to collect COFs materials; the polymerization agent is at least one of peracetic acid, dibenzoyl peroxide, isonicotinic anhydride, angelic anhydride, benzoic anhydride, azobenzene, and azobisisobutyronitrile;
[0014] 2) COFs washing and drying: The prepared COFs material is fully washed with a washing agent to remove impurities, and then dried to obtain the COFs material;
[0015] 3) COFs acid modification: COFs material and organic solvent are mixed and cooled in an ice bath; then the acidifying agent and organic solvent are added dropwise to the COFs suspension and stirred at room temperature for 10-50h, and then the mixture is added to deionized water at 0-5°C, and the solid is collected after thorough washing and dried to obtain the acid-modified COFs material;
[0016] 4) Acid-modified COFs loaded with metal: The acid-modified COFs material and the solvent are mixed, and the metal compound solution is added after being evenly dispersed. After being evenly dispersed again, the mixture is immersed for 10-50 hours under stirring, and finally the system solvent is removed and dried to obtain product 1;
[0017] 5) Calcination and reduction: The product 1 is placed in a tubular furnace, and an inert gas is first introduced into the tubular furnace, and calcined at high temperature under the protection of the inert gas. After cooling, hydrogen is introduced, and high-temperature reduction is performed under a H2 atmosphere. The solid is then cooled to room temperature to obtain an acid-modified supported COFs catalyst.
[0018] Preferably, the pyridine compound in step 1) is at least one of 2,4,6-trimethoxypyridine, 2,4,6-trimethylpyridine, 2,4,6-tribromopyridine, 2,4,6-triphenylpyridine, 2,4,6-tri(3-bromophenyl)pyridine, and 3-acetyl-2,4,6-trimethylpyridine; and the aldehyde compound is at least one of adipaldehyde, succinaldehyde, isophthalaldehyde, biphenyldicarboxaldehyde, terephthalaldehyde, triacetaldehyde, and trioxymethylene.
[0019] Preferably, in step 1), the molar ratio of the pyridine compound to the aldehyde compound is 1:0.5-1:3, more preferably 1:1-2, and even more preferably 1:1.5. The molar ratio of the pyridine compound to the polymerization agent is 1:1-2, preferably 1:1.
[0020] Preferably, in step 1), the reaction temperature is 150-200°C, more preferably 170-190°C, and further preferably 180°C; the reaction time is 30-120h, more preferably 70-80h, and further preferably 72h.
[0021] Preferably, the washing reagent in step 2) is at least one of deionized water, methanol, ethanol, acetonitrile, acetone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0022] Preferably, in step 2), the drying temperature is 50° C.-150° C., more preferably 100° C.; the drying time is 10-15 h, more preferably 12 h.
[0023] Preferably, the organic solvent in step 3) is at least one of methanol, toluene, acetone, dichloromethane, cyclohexane and ethyl acetate.
[0024] Preferably, the acidifying agent in step 3) is at least one of hydrochloric acid, chlorosulfonic acid, aminosulfonic acid, glacial acetic acid, oxalic acid, and phosphotungstic acid, and more preferably chlorosulfonic acid.
[0025] Preferably, in step 3), the mass amount of the acidifying agent is 5-40% of the total mass amount of the COFs material and the acidifying agent, and more preferably 20-30%.
[0026] Preferably, the stirring time in step 3) is 20-30 h, more preferably 24 h.
[0027] Preferably, in step 3), the drying temperature is 50° C.-150° C., more preferably 100° C.; the drying time is 5-15 h, more preferably 10 h.
[0028] Preferably, the solvent in step 4) is at least one of deionized water, methanol, ethanol, propanol and acetone, preferably a mixed solvent of deionized water and ethanol, more preferably a volume ratio of deionized water to ethanol is 1:1.
[0029] Preferably, the metal in step 4) is at least one of copper, iron, nickel, platinum, palladium, ruthenium and iridium.
[0030] Preferably, in step 4), the metal loading is 1-10 wt %, more preferably 5 wt %, and the metal loading refers to the mass ratio of the metal element used to the carrier.
[0031] Preferably, the stirring and immersion time in step 4) is 20-30 hours, more preferably 24 hours.
[0032] Preferably, in step 4), the drying temperature is 50° C.-100° C., more preferably 80° C.; the drying time is 1-3 h, more preferably 2 h.
[0033] Preferably, in step 5), the calcination temperature is 250° C.-400° C., more preferably 300° C.; the calcination time is 1-5 h, more preferably 2 h.
[0034] Preferably, in step 5), the reduction temperature is 250° C.-400° C., more preferably 300° C.; the reduction time is 1-5 h, more preferably 2 h.
[0035] In a second aspect, the present invention provides an acid-modified supported COFs catalyst prepared according to the preparation method described in the first aspect.
[0036] In a third aspect, the present invention provides an application of the acid-modified supported COFs catalyst described in the second aspect in the alkylanilation reaction of nitrobenzene compounds, wherein the alkylanilation reaction of nitrobenzene compounds uses nitrobenzene compounds, ketone compounds and hydrogen as raw materials, and adopts a one-pot method to react without the need for additional addition of an acidic reagent, and the ketone compound is a dialkyl ketone or a cycloalkyl ketone.
[0037] In a specific embodiment of the present invention, the benzene ring of the nitrobenzene compound may not contain other substituents, or may contain at least one substituent, and the substituent may be a C1-C10 alkyl group, specifically 3,4-dimethylnitrobenzene, p-nitrotoluene, o-nitroethylbenzene, 3-nitro-o-xylene, etc. The ketone compound is a dialkyl ketone or a cycloalkyl ketone, and the two alkyl groups in the dialkyl ketone may be the same or different, and the alkyl group may be selected from C1-C10 alkyl groups, specifically 2-pentanone, 3-pentanone, methyl ethyl ketone, 3-hexanone, etc.; the cycloalkyl group may be a 5-7-membered ring, and the cycloalkyl group may not contain other substituents, or may contain at least one substituent, such as a C-C4 alkyl group, and a typical example of the cycloalkyl ketone is cyclohexanone. Taking the alkylanilinization reaction of 3,4-dimethylnitrobenzene and 3-pentanone in a hydrogen atmosphere to generate N-(1-ethylpropyl)-3,4-dimethylaniline as an example, the reaction process is as follows:
[0038]
[0039] Preferably, the molar ratio of the nitrobenzene compound to the ketone compound is 1:1-1:3, more preferably 1:2.
[0040] Preferably, the hydrogen pressure in the reaction is 1.5-3MPa, more preferably 2-3MPa, and further preferably 2.5MPa; the reaction temperature is 80°C-150°C, further preferably 90-110°C, and further preferably 100°C; the reaction time is 1-10h, further preferably 5-10h, and further preferably 8h.
[0041] The acidic reagent described in the present invention refers to liquid acid, solid acid, etc. that need to be added in the conventional alkylanilinization reaction of nitrobenzene compounds.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] 1) The present invention uses COFs materials to replace traditional carriers, making full use of the structural advantages of COFs such as high specific surface area, regular pore structure, thermal stability and chemical stability, thereby improving the catalytic performance of the active center.
[0044] 2) The present invention uses a grafting method to externally add acidic functional groups, so that the catalyst has an acid catalytic function, which gets rid of the method of adding an acidic reagent in the traditional process, improves resource utilization and reduces process costs, and is in line with the general trend of green pesticides.
[0045] 3) In the loading stage of the present invention, metal nanoparticles can be loaded inside the pores through the highly ordered pore structure of the COFs material, and the metal has a high dispersion and is not easy to agglomerate, which can improve the selectivity and stability of the reaction.
[0046] 4) The catalyst prepared by the present invention is used in the amination of alkylanilines of nitrobenzene compounds, and the reaction has high conversion rate, high selectivity and high stability, and has broad industrial application prospects. DETAILED DESCRIPTION
[0047] In order to better understand the technical solution of the present invention, the technical solution provided by the present invention is described in detail below in conjunction with specific embodiments, but the scope of protection claimed in the present invention is not limited to the scope described in the embodiments.
[0048] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained by conventional technical means or purchased commercially.
[0049] Catalyst Preparation Example 1
[0050] COFs synthesis: 2,4,6-trimethylpyridine (15mmol), benzoic anhydride (15mmol) and terephthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 72h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was dried at 100℃ for 12h to obtain the material.
[0051] Catalyst preparation: 2 g COFs were added to 40 mL dry dichloromethane and cooled in an ice bath. 0.303 mL chlorosulfonic acid and 10 mL dry dichloromethane were added dropwise to the COFs suspension and stirred at room temperature for 24 hours. The mixture was then added to ice water, washed thoroughly, and dried at 100 °C for 10 hours to obtain COF-SO3H material.
[0052] Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment for about 25min again, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After passing Ar / N2 for 0.5h, calcine at 300℃ argon / nitrogen for 2h, then cool and reduce with H2 at 300℃ for 2h, and then cool the solid to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0053] 32.3428 g of a mixed solution of 3,4-dimethylnitrobenzene and 3-pentanone (molar ratio of 1:2) was added to the reactor and reacted at 100°C and 2.5 MPa H2 atmosphere for 8 hours. After the reaction, the reactant conversion rate was measured to be 99.96% and the product selectivity was 97.27%.
[0054] Catalyst Preparation Example 2
[0055] COFs synthesis: 2,4,6-trimethylpyridine (15mmol), benzoic anhydride (15mmol) and terephthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 120h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was dried at 100℃ for 12h to obtain the material.
[0056] Catalyst preparation: 2 g COFs were added to 40 mL dry dichloromethane and cooled in an ice bath. 0.303 mL chlorosulfonic acid and 10 mL dry dichloromethane were added dropwise to the COFs suspension and stirred at room temperature for 24 hours. The mixture was then added to ice water, washed thoroughly, and dried at 100 °C for 10 hours to obtain COF-SO3H material.
[0057] Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment for about 25min again, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After passing Ar / N2 for 0.5h, calcine at 300℃ argon / nitrogen for 2h, then cool and reduce with H2 at 300℃ for 2h, and then cool the solid to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0058] 33.1435 g of a mixed solution of 3,4-dimethylnitrobenzene and methyl ethyl ketone (molar ratio of 1:2.5) was added to the reactor and reacted at 100°C and 2.5 MPa H2 atmosphere for 8 hours. After the reaction, the reactant conversion rate was measured to be 94.36% and the product selectivity was 95.87%.
[0059] Catalyst Preparation Example 3
[0060] COFs synthesis: 2,4,6-trimethylpyridine (15mmol), benzoic anhydride (15mmol) and terephthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 150℃ and reacted for 36h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was dried at 100℃ for 12h to obtain the material.
[0061] Catalyst preparation: 2 g COFs were added to 40 mL dry dichloromethane and cooled in an ice bath. 0.303 mL chlorosulfonic acid and 10 mL dry dichloromethane were added dropwise to the COFs suspension and stirred at room temperature for 24 hours. The mixture was then added to ice water, washed thoroughly, and dried at 100 °C for 10 hours to obtain COF-SO3H material.
[0062] Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment for about 25min again, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After passing Ar / N2 for 0.5h, calcine at 300℃ argon / nitrogen for 2h, then cool and reduce with H2 at 300℃ for 2h, and then cool the solid to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0063] 32.3428 g of a mixed solution of 3,4-dimethylnitrobenzene and 3-pentanone (molar ratio of 1:2) was added to the reactor and reacted at 100°C and 2.5 MPa H2 atmosphere for 8 hours. After the reaction, the conversion rate of the reactants was measured to be 87.73% and the product selectivity was 98.81%.
[0064] Catalyst Preparation Example 4
[0065] COFs synthesis: 2,6-dimethylpyridine (15mmol), peracetic acid (15mmol) and isophthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 72h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was obtained by drying at 100℃ for 12h.
[0066] Catalyst preparation: Add 2g COFs to 40mL dry acetone and cool in an ice bath. Add 0.5312g aminosulfonic acid and 10mL dry acetone to the COFs suspension, stir at room temperature for 24 hours, then add the mixture to ice water, wash thoroughly, and dry at 100℃ for 10h to obtain COF-SO3H material. Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment again for about 25min, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After passing Ar / N2 for 0.5 h, the solid was calcined at 300 °C under argon / nitrogen for 2 h, cooled and reduced with H2 at 300 °C for 2 h, and then cooled to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0067] 32.3428 g of a mixed solution of 3,4-dimethylnitrobenzene and 3-pentanone (molar ratio of 1:2) was added to the reactor and reacted at 100°C and 2.5 MPa H2 atmosphere for 8 hours. After the reaction, the conversion rate of the reactants was measured to be 94.57% and the product selectivity was 89.31%.
[0068] Catalyst Preparation Example 5
[0069] COFs synthesis: 2,4,6-trimethoxypyridine (15mmol), isonicotinic anhydride (15mmol) and adipaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 72h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylacetamide and methanol. The material was dried at 100℃ for 12h to obtain the material.
[0070] Catalyst preparation: 2g COFs was added to 40mL methanol, and then 0.5312g phosphotungstic acid and 10mL methanol were added to the COFs suspension, stirred at room temperature for 24 hours, and then the mixture was poured into deionized water, washed thoroughly, and dried at 100℃ for 10h to obtain COF-HPW material. 2g COF-HPW was dispersed in a 100mL round-bottom flask, and then 20mL ethanol and 20mL water were added to the vial in sequence. After ultrasonic treatment for about 25min, 2.11mL of hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL was added, and ultrasonic treatment was performed again for about 25min, stirred at 400r / min for 24h, and finally the system solvent was removed by rotary evaporation (40℃), and dried at 80℃ for 2h. After passing Ar / N2 for 0.5 h, the solid was calcined at 300 °C under argon / nitrogen for 2 h, cooled and reduced with H2 at 300 °C for 2 h, and then cooled to room temperature to obtain the desired Pt@COF-HPW with COFs as the carrier.
[0071] 32.3428 g of a mixed solution of 3,4-dimethylnitrobenzene and 3-pentanone (molar ratio of 1:2) was added to the reactor and reacted at 100°C and 2.5 MPa H2 atmosphere for 8 hours. After the reaction, the conversion rate of the reactants was measured to be 67.38% and the product selectivity was 79.95%.
[0072] Substrate applicable example 1
[0073] COFs synthesis: 2,4,6-trimethylpyridine (15mmol), benzoic anhydride (15mmol) and terephthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 36h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was obtained by drying at 100℃ for 12h.
[0074] Catalyst preparation: Add 2g COFs to 40mL dry dichloromethane and cool in an ice bath. Add 0.303mL chlorosulfonic acid and 10mL dry dichloromethane dropwise to the COFs suspension, stir at room temperature for 24 hours, then add the mixture to ice water, wash thoroughly, and dry at 100℃ for 10h to obtain COF-SO3H material. Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL of hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment again for about 25min, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After Ar / N2 was introduced for 0.5 h, the mixture was calcined at 300 °C under argon / nitrogen for 2 h, cooled, and reduced with H2 at 300 °C for 2 h. The solid was then cooled to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0075] 39.5538 g of a mixed solution of p-nitrotoluene and 3-pentanone (molar ratio of 1:3) was added to the reactor and reacted at 80°C and 2.5 MPa H2 atmosphere for 6 hours. After the reaction, the reactant conversion rate was measured to be 99.51% and the product selectivity was 95.32%.
[0076] Substrate applicable example 2
[0077] COFs synthesis: 2,4,6-trimethylpyridine (15mmol), benzoic anhydride (15mmol) and terephthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 72h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was dried at 100℃ for 12h to obtain the material.
[0078] Catalyst preparation: Add 2g COFs to 40mL dry dichloromethane and cool in an ice bath. Add 0.303mL chlorosulfonic acid and 10mL dry dichloromethane dropwise to the COFs suspension, stir at room temperature for 24 hours, then add the mixture to ice water, wash thoroughly, and dry at 100℃ for 10h to obtain COF-SO3H material. Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL of hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment again for about 25min, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After Ar / N2 was introduced for 0.5 h, the mixture was calcined at 300 °C under argon / nitrogen for 2 h, cooled, and reduced with H2 at 300 °C for 2 h. The solid was then cooled to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0079] 32.3423 g of a mixed solution of o-nitroethylbenzene and 2-pentanone (molar ratio of 1:2) was added to the reactor and reacted at 80°C and 2.5 MPa H2 atmosphere for 8 hours. After the reaction, the conversion rate of the reactants was measured to be 98.98% and the product selectivity was 91.33%.
[0080] Substrate applicable example 3
[0081] COFs synthesis: 2,4,6-trimethylpyridine (15mmol), benzoic anhydride (15mmol) and terephthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 72h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was dried at 100℃ for 12h to obtain the material.
[0082] Catalyst preparation: Add 2g COFs to 40mL dry dichloromethane and cool in an ice bath. Add 0.303mL chlorosulfonic acid and 10mL dry dichloromethane dropwise to the COFs suspension, stir at room temperature for 24 hours, then add the mixture to ice water, wash thoroughly, and dry at 100℃ for 10h to obtain COF-SO3H material. Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL of hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment again for about 25min, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After Ar / N2 was introduced for 0.5 h, the mixture was calcined at 300 °C under argon / nitrogen for 2 h, cooled, and reduced with H2 at 300 °C for 2 h. The solid was then cooled to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0083] 29.536 g of a mixture of 3-nitro-o-xylene and methyl ethyl ketone (molar ratio of 1:2) was added to the reactor and reacted at 100°C and 2.5 MPa H2 atmosphere for 6 hours. After the reaction, the reactant conversion rate was measured to be 99.27% and the product selectivity was 89.77%.
[0084] Long cycle implementation
[0085] COFs synthesis: 2,4,6-trimethylpyridine (15mmol), benzoic anhydride (15mmol) and terephthalaldehyde (22.5mmol) were added to the reactor respectively. After freezing the reactor in liquid nitrogen, the reactor was sealed and evacuated until the pressure was below 50 mTorr; then the reactor was heated to 180℃ and reacted for 72h, and then the COFs material was collected after opening the reactor. Then it was washed with N,N-dimethylformamide and methanol. The material was dried at 100℃ for 12h to obtain the material.
[0086] Catalyst preparation: Add 2g COFs to 40mL dry dichloromethane and cool in an ice bath. Add 0.303mL chlorosulfonic acid and 10mL dry dichloromethane dropwise to the COFs suspension, stir at room temperature for 24 hours, then add the mixture to ice water, wash thoroughly, and dry at 100℃ for 10h to obtain COF-SO3H material. Take 2g COF-SO3H and disperse it in a 100mL round-bottom flask, then add 20mL ethanol and 20mL water to the vial in turn. After ultrasonic treatment for about 25min, add 2.11mL of hexahydrate chloroplatinic acid solution with a platinum content of 0.05g / mL, ultrasonic treatment again for about 25min, stir at 400r / min for 24h, and finally remove the system solvent by rotary evaporation (40℃), and dry at 80℃ for 2h. After Ar / N2 was introduced for 0.5 h, the mixture was calcined at 300 °C under argon / nitrogen for 2 h, cooled, and reduced with H2 at 300 °C for 2 h. The solid was then cooled to room temperature to obtain the desired Pt@COF-SO3H with COFs as the carrier.
[0087] 32.3428 g of a mixed solution of 3,4-dimethylnitrobenzene and 3-pentanone (molar ratio of 1:2) was added to the reactor, and the reaction was carried out at 100°C and 2.5 MPa H2 atmosphere for 120 hours. After the reaction, the reactant conversion rate and product selectivity were measured as shown in Table 1 below:
[0088] Table 1
[0089]
Claims
1. A method for preparing an acid-modified supported COFs catalyst, characterized in that: The preparation method is carried out according to the following steps: 1) Preparation of COFs: Pyridine compounds and aldehyde compounds are added to a reactor respectively, mixed evenly, and then a polymerization agent is added; the reactor is placed in liquid nitrogen for freezing, and then the reactor is sealed and evacuated until the pressure is displayed below 50 mTorr; then the temperature is raised to 120°C-200°C for reaction for 10-100 hours, and finally the reactor is opened to collect COFs materials; the polymerization agent is at least one of peracetic acid, dibenzoyl peroxide, isonicotinic anhydride, angelic anhydride, benzoic anhydride, azobenzene, and azobisisobutyronitrile; 2) COFs washing and drying: The prepared COFs material is fully washed with a washing agent to remove impurities, and then dried to obtain the COFs material; 3) COFs acid modification: COFs material and organic solvent are mixed and cooled in an ice bath; then the acidifying agent and organic solvent are added dropwise to the COFs suspension and stirred at room temperature for 10-50h, and then the mixture is added to deionized water at 0-5°C, and the solid is collected after thorough washing and dried to obtain the acid-modified COFs material; 4) Acid-modified COFs loaded with metal: The acid-modified COFs material and the solvent are mixed, and the metal compound solution is added after being evenly dispersed. After being evenly dispersed again, the mixture is immersed for 10-50 hours under stirring, and finally the system solvent is removed and dried to obtain product 1; 5) Calcination and reduction: The product 1 is placed in a tubular furnace, and an inert gas is first introduced into the tubular furnace, and calcined at high temperature under the protection of the inert gas. After cooling, hydrogen is introduced, and high-temperature reduction is performed under a H2 atmosphere. The solid is then cooled to room temperature to obtain an acid-modified supported COFs catalyst.
2. The preparation method according to claim 1, characterized in that: The pyridine compound in step 1) is at least one of 2,4,6-trimethoxypyridine, 2,4,6-trimethylpyridine, 2,4,6-tribromopyridine, 2,4,6-triphenylpyridine, 2,4,6-tri(3-bromophenyl)pyridine, and 3-acetyl-2,4,6-trimethylpyridine; the aldehyde compound is at least one of adipaldehyde, succinaldehyde, isophthalaldehyde, biphenyldicarboxaldehyde, terephthalaldehyde, triacetaldehyde, and trioxymethylene; The molar ratio of the pyridine compound to the aldehyde compound is 1:0.5-1:3, more preferably 1:1-2, and even more preferably 1:1.5; the molar ratio of the pyridine compound to the polymerization agent is 1:1-2, and preferably 1:
1.
3. The preparation method according to claim 1, characterized in that: In step 1), the reaction temperature is 150-200°C, more preferably 170-190°C, and more preferably 180°C; the reaction time is 30-120h, more preferably 70-80h, and more preferably 72h.
4. The preparation method according to claim 1, characterized in that: In step 3), the organic solvent is at least one of methanol, toluene, acetone, dichloromethane, cyclohexane, and ethyl acetate; the acidifying agent is at least one of hydrochloric acid, chlorosulfonic acid, aminosulfonic acid, glacial acetic acid, oxalic acid, and phosphotungstic acid, and the mass amount of the acidifying agent is 5-40% of the total mass amount of the COFs material and the acidifying agent, and more preferably 20-30%.
5. The preparation method according to claim 1, characterized in that: The stirring time in step 3) is 20-30 hours, more preferably 24 hours.
6. The preparation method according to claim 1, characterized in that: In step 4), the solvent is at least one of deionized water, methanol, ethanol, propanol, and acetone, preferably a mixed solvent of deionized water and ethanol; and the metal is at least one of copper, iron, nickel, platinum, palladium, ruthenium, and iridium.
7. The preparation method according to claim 1, characterized in that: In step 4), the metal loading is 1-10 wt %, more preferably 5 wt %, and the metal loading refers to the mass ratio of the metal element used to the carrier.
8. The preparation method according to claim 1, characterized in that: In step 5), the calcination temperature is 250°C-400°C, more preferably 300°C; the calcination time is 1-5h, more preferably 2h; In step 5), the reduction temperature is 250°C-400°C, more preferably 300°C; the reduction time is 1-5h, more preferably 2h.
9. An acid-modified supported COFs catalyst prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the acid-modified supported COFs catalyst as claimed in claim 9 in the alkylanilation reaction of nitrobenzene compounds, wherein the alkylanilation reaction of nitrobenzene compounds uses nitrobenzene compounds, ketone compounds and hydrogen as raw materials, and adopts a one-pot process to react without the need for additional addition of an acidic reagent, and the ketone compound is a dialkyl ketone or a cycloalkyl ketone.