Modified layered metal hydroxide composite catalytic material as well as preparation method and application thereof
By growing layered metal hydroxides on nitrogen-doped open hollow carbon, the electrostatic agglomeration problem of catalytic materials is solved, the active site and stability are improved, and efficient persulfate activation and iodine X-ray contrast agent are achieved. The degradation of the dynamism solves the problem of the activation process and the secondary pollution in traditional technology.
Patent Information
- Application Number
- CN202410560768.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-12
AI Technical Summary
The existing layered metal hydroxide catalytic materials are prone to electrostatic agglomeration, resulting in fewer active sites. Traditional advanced oxidation technology takes a long time to activate persulfate, has secondary pollution and requires a large amount of energy, making it difficult to effectively degrade iodine. Organic pollutants such as X-ray contrast agents.
By growing layered metal hydroxides on the support nitrogen-doped open hollow carbon, the conductivity and active sites of the material are increased, and modified catalytic materials are prepared by solvent-thermal synthesis method, and metal particles are fixed using nitrogen elements to improve material stability and specific surface area, optimize the activation process of persulfate.
Effectively avoid metal agglomeration problems, increase the conductivity and active sites of the material, improve the degradation rate of pollutants, achieve efficient activation of persulfate, achieve 100%, and maintain good results in multiple cycles. stability.
Smart Images

Figure CN118925809A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a catalytic material, in particular to a modified layered metal hydroxide composite catalytic material and a preparation method and application thereof. Background Art
[0002] The increasing shortage of freshwater resources is a global challenge. With the rapid development of the times, further urbanization and socialization have led to an increase in the use of medicines and personal care products. Most medicines and personal care products have a low detection limit in the environment and are difficult to remove from water bodies through traditional water treatment methods due to their complex structures. This leads to their long-term presence in water bodies and finally their enrichment in the human body with water circulation, which can cause irreversible damage to the human body. As one of the diagnostic drugs, iodinated X-ray contrast agents have been used more and more year by year due to the continuous increase in the incidence of various chronic and complex diseases and the increase in the number of medical diagnostic tests. In order to ensure imaging contrast, they are designed to be inert and highly soluble drugs that are difficult to remove from water bodies. Diatrizoic acid (DTZ), as the most widely used iodinated X-ray contrast agent, has a nephrotoxic effect on the human body on the one hand, and can be converted into more toxic disinfection byproducts during the disinfection of drinking water, which has extremely strong cytotoxicity and genotoxicity.
[0003] Advanced oxidation technology (AOPs) is a technology that oxidizes macromolecular refractory organic matter into low-toxic or non-toxic small molecules under reaction conditions such as high temperature and high pressure, electricity, sound, light irradiation, and catalysts. Its advantage is that it can generate active species to ultimately degrade refractory pollutants into non-toxic small molecules such as carbon dioxide or water molecules; in addition, it is simple to operate, has little secondary pollution, and has mild reaction conditions and high efficiency. However, the traditional advanced oxidation technology has been hindered from being widely applicable due to its shortcomings such as short life and low selectivity, narrow working pH range, unfriendly cost, and poor stability. The persulfate advanced oxidation technology can produce sulfate radicals with strong oxidation potential and longer service life through a variety of activation methods. In addition, its wide pH range and easy storage and transportation have attracted widespread attention from scholars. Persulfate (PMS) has a longer OO bond and an asymmetric structure, which is easier to be activated than persulfate (PDS), producing more active substances. However, existing activation technologies are usually time-consuming, have secondary pollution, and require a lot of energy. Transition metal-based heterogeneous catalysts have attracted much attention due to their advantages such as good catalytic effect, low cost, and easy recovery. This technology has certain disadvantages. Single metal catalysts often lose their activity due to inefficient conversion from high-valent to low-valent. Leaching of toxic metals caused by unstable crystal structures has become a huge obstacle to the practical application of these transition metal catalysts.
[0004] Layered double hydroxide (LDH) is a two-dimensional anionic clay material with a layered structure consisting of two layers of metal hydroxides. The interlayer is composed of positively charged octahedral metal hydroxides, in which negative anions and water molecules are sandwiched in a repetitive manner between the positively charged metal layers to maintain electrical neutrality. Due to the high tunability of metal ions in the main layer, it has attracted widespread attention as a catalyst. The introduction of transition metals enables electron transfer between different metals to accelerate the valence cycle. In addition, the introduction of foreign metals can also improve the stability of heterogeneous catalysts and reduce the leaching of toxic metal ions. The advantages of this material are (1) low cost and simple production process (2) flexible chemical composition, and a variety of transition metals and functional anions can be used to prepare LDH to enhance catalytic performance (3) stable structure and good fixation effect on toxic metal ions (4) diverse morphology, which can be easily changed by calcination and other methods, thereby exposing more active sites. LDH has been widely used in catalysis, energy storage, medical treatment, sensing and other fields. However, existing LDH catalytic materials are prone to electrostatic aggregation. Summary of the invention
[0005] Purpose of the invention: The first purpose of the present invention is to provide a modified layered metal hydroxide composite catalytic material to improve the problem of easy electrostatic agglomeration of layered metal hydroxides; the second purpose of the present invention is to provide a method for preparing the layered metal hydroxide; the third purpose of the present invention is to provide the application of the layered metal hydroxide in activating persulfate to degrade organic dyes.
[0006] Technical solution: The modified layered metal hydroxide composite catalytic material of the present invention comprises a carrier nitrogen-doped open hollow carbon and a metal hydroxide loaded on the carrier.
[0007] Layered metal hydroxides grow vertically on the inner and outer surfaces of open hollow carbon, which solves the problem of fewer active sites caused by the easy agglomeration of metals in LDH itself. In addition, the conductivity of the material is increased and the active sites are increased. According to relevant electrochemical characterizations, the material's electron transfer internal resistance, charge response and electrochemical active area have all been improved to a certain extent.
[0008] Preferably, the open hollow carbon is doped with nitrogen. The nitrogen element is introduced into the open hollow carbon to fix the metal particles, making it difficult for metal ions to precipitate, improving the material stability, increasing the specific surface area of the material, and providing more active sites.
[0009] Preferably, the metals are nickel, cobalt and iron, wherein the molar ratio of nickel, cobalt and iron is 1:1:1 to 1:3:3.
[0010] The method for preparing the layered metal hydroxide composite catalytic material of the present invention comprises the following steps:
[0011] (1) mixing the open hollow carbon with a nitrogen source and bicarbonate, and then calcining at a high temperature to obtain nitrogen-doped open hollow carbon;
[0012] (2) dissolving the metal salt and urea in a solvent, adding nitrogen-doped open hollow carbon to obtain a suspension, and performing a solvent thermal synthesis reaction to obtain the layered metal hydroxide composite catalytic material.
[0013] In step (1), the introduction of nitrogen can provide alkaline surface functional groups, which can improve the surface interaction of carbon. On the one hand, it fixes the metal particles and makes it difficult for metal ions to precipitate. On the other hand, it provides a faster basis for electron transfer and improves the stability of the material.
[0014] Preferably, in step (1), the mass ratio of the open hollow carbon to the nitrogen source and the bicarbonate is 1:0:4 to 1:8:4. The content of N element added varies with the mass of the nitrogen source. Too little nitrogen content has little effect on the improvement of the material; when the nitrogen content increases, on the one hand, the metal stability of the material is increased, and secondly, the catalytic activity of the base carbon material can be accelerated; adding too much will cause the stability of the material to decrease.
[0015] Preferably, in step (1), the nitrogen source is ammonium oxalate monohydrate; and the bicarbonate is potassium bicarbonate or sodium bicarbonate.
[0016] Preferably, in step (1), the high temperature calcination temperature is 800-1000°C.
[0017] Preferably, in step (2), the solvent is ethanol, and the solvent thermal reaction temperature is 100-160° C. Due to its unique properties, such as low boiling point and relatively high polarization, ethanol changes the surface energy of the crystal and reduces the crystal growth rate, thereby forming a flower-like microsphere structure.
[0018] The role of urea: providing carbonate ions (water generated by the reaction of ethanol reacts with carbonate to generate hydroxide) and an alkaline environment, the pH value rises slowly, and agglomeration is reduced.
[0019] In step (2), the metal salt is a nickel salt, a cobalt salt and an iron salt. Preferably, the nickel salt is one of nickel chloride, nickel sulfate, nickel nitrate or nickel hydroxide. Preferably, the cobalt salt is one of cobalt nitrate, cobalt sulfate or cobalt chloride. Preferably, the iron salt is one of ferric chloride, ferric sulfate or ferric nitrate.
[0020] Preferably, the preparation method of the open hollow carbon is: pre-mixing two soft templates of sodium dodecyl sulfate and block polyether P123, adding a carbon source, and then performing a hydrothermal carbonization reaction, and obtaining the open hollow carbon after the reaction is completed.
[0021] Sodium dodecyl sulfate (CAS: 151-21-3) was purchased from Aladdin. Block polyether P123 (CAS: 9003-11-6) was purchased from Dulai Biotechnology.
[0022] Preferably, the molar ratio of sodium dodecyl sulfate to block polyether P123 is 1:1 to 5. Sodium dodecyl sulfate and block polyether P123 are used as soft templates to form mixed micelles in aqueous solution through hydrophobic interactions. Then, during the hydrothermal reaction, ribose is polymerized on the template to form an oligomer carbon shell. P123 promotes the dispersion of the nanoemulsion. When the amount of P123 is zero, the prepared material is not open at this time; when the amount of P123 is increased, when the hydrothermal temperature is higher than 100°C, the poly (ethylene glycol) block of P123 causes the volume of the internal emulsion to expand, thereby generating tensile stress from the inside to the outside. When the expansion pressure exceeds the critical value, the oligomer shell ruptures, and the internal microemulsion flows out, resulting in the re-formation of the opening on the surface, and when the P123 content increases, the pressure increases, thereby providing control over the opening diameter.
[0023] Preferably, the temperature of the hydrothermal carbonization reaction is 150-200° C. When the hydrothermal temperature is too low, the yield of the prepared material is small and a spherical structure cannot be formed; when the reaction temperature is further increased, the material yield increases, and the crystal nuclei are more likely to collide and combine with each other, so the carbon microspheres are seriously cross-linked, and the particle size is large and unevenly distributed.
[0024] Preferably, the reaction time is 8 to 24 hours. When the hydrothermal time is too short, most of the solution in the reactor is still in the form of an emulsion, and only a small part can form a spherical structure. At this time, the carbon output is small and it is difficult to form an open structure; as the reaction time increases, after the spherical carbon opens, the emulsion inside the sphere will flow out and continue to polymerize at the opening and inside. At this time, the thickness of the sphere will increase, and a neck-like structure will gradually form at the opening.
[0025] Preferably, the carbon source is D-(-)-ribose.
[0026] The LDH composite catalytic material of the present invention is used in activating persulfate to degrade organic pollutants.
[0027] Preferably, the organic pollutant is an iodinated X-ray contrast agent.
[0028] Invention mechanism: The present invention uses nitrogen-doped open carbon as the substrate, and layered metal hydroxide grows on the inner and outer surfaces of the material in a vertical growth manner, which solves the problem of fewer active sites caused by the easy agglomeration of metals in LDH itself. In addition, the conductivity of the material is increased, and the active sites are increased. According to relevant electrochemical characterization, the electron transfer internal resistance, charge response and electrochemical active area of the material have been improved to a certain extent. In addition, the pore-forming nitrogen-doping step is carried out. The purpose of adding bicarbonate is to further increase the relative specific surface area of the material and provide more active sites for reaction. The added nitrogen atoms have a new effect on the catalytic performance of metal / nitrogen-doped porous carbon composite materials. On the one hand, nitrogen-containing groups can serve as active sites for the nucleation and growth of metal nanoparticles, which can stabilize the deposited small-sized and narrowly distributed metal nanoparticles; through the electronic interaction between metal nanoparticles and the carrier, N atoms can significantly affect the chemical state of the loaded metal nanoparticles; on the other hand, metal-nitrogen bonding can be formed, which can help fix the metals in their original positions, thereby inhibiting their mobility.
[0029] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The modified layered metal hydroxide composite catalytic material avoids the problem of metal agglomeration by vertically growing LDH on the inner and outer surfaces of nitrogen-doped open hollow carbon, thereby increasing the conductivity of the material and increasing the active sites; (2) The modified layered metal hydroxide composite catalytic material fixes the metal particles by introducing nitrogen elements on the open hollow carbon, making it difficult for metal ions to precipitate, thereby improving the stability of the material, and increasing the specific surface area of the material, providing more active sites; (3) The preparation method is simple and easy to industrialize; (4) The modified layered metal hydroxide composite catalytic material is used to activate persulfate to degrade organic pollutants, thereby achieving efficient activation of persulfate and improving the degradation rate of pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A comparison chart of the treatment effects of catalytic materials prepared in Examples 1 to 5 of the present invention and Comparative Example 1 on diatrizoate wastewater;
[0031] Figure 2 This is a comparison chart of the treatment effects of catalytic materials of Example 1 and Examples 6 to 9 of the present invention on diatrizoate wastewater;
[0032] Figure 3 This is a comparison chart of the treatment effects of adding different materials on diatrizoate wastewater;
[0033] Figure 4 A comparison chart showing the effect of repeatedly using the catalytic material prepared in Example 1 of the present invention on treating diatrizoate wastewater;
[0034] Figure 5This is a SEM image of the open hollow carbon prepared in Example 1 of the present invention;
[0035] Figure 6 These are the SEM and mapping images of the catalytic material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is further described below in conjunction with embodiments.
[0037] Example 1
[0038] The modified layered metal hydroxide composite catalytic material of the present invention comprises the following steps:
[0039] (1) Sodium dodecyl sulfate and block polyether P123, two soft templates, were dissolved in ultrapure water at a molar ratio of 1:2 and stirred for 30 min, 0.5 mol / L carbon source was added and stirred for 30 min, and then placed in an oven for hydrothermal carbonization at 180° C. for 16 h. After the reaction was completed, the product was centrifuged and washed and dried;
[0040] (2) grinding the open hollow carbon obtained in step (1) with ammonium oxalate monohydrate and potassium bicarbonate in a mass ratio of 1:4:4 until the mixture is uniformly mixed, and placing the ground material in a tube furnace for further reaction;
[0041] (3) The material fired in step (2) was acid-washed for 12 hours, then washed with water and dried in an oven;
[0042] (4)(1) Weigh 3.635 mg (0.25 mM) Ni(NO3)2·6H2O, 10.91 mg (0.75 mM) Co(NO3)2·6H2O and 10.1 mg (0.5 mM) Fe(NO3)3·9H2O and dissolve them in 50 ml of ethanol solution, add 1 g of urea, stir until completely dissolved, add 50 mg of the homemade carbon material, stir evenly and set aside;
[0043] (5) The mixed solution of step (4) is added into an autoclave, and a hydrothermal synthesis reaction is carried out at 120° C. for 12 h. After the reaction is completed, the composite material obtained in the above process is taken out, filtered, repeatedly washed with ultrapure water and ethanol solution, and then placed in an oven for drying at 60° C. to obtain the modified layered metal hydroxide composite catalytic material.
[0044] Example 2
[0045] On the basis of Example 1, the hydrothermal carbonization time in step (1) was changed to 8 h, and the other conditions remained unchanged.
[0046] Example 3
[0047] On the basis of Example 1, the hydrothermal carbonization time in step (1) was changed to 12 h, and the other conditions remained unchanged.
[0048] Example 4
[0049] On the basis of Example 1, the hydrothermal carbonization time in step (1) was changed to 20 h, and the other conditions remained unchanged.
[0050] Example 5
[0051] On the basis of Example 1, the hydrothermal carbonization time in step (1) was changed to 24 h, and the other conditions remained unchanged.
[0052] Example 6
[0053] On the basis of Example 1, the mass ratio of the open hollow carbon to ammonium oxalate monohydrate and potassium bicarbonate in step (2) was changed to 1:0:4, and the other conditions remained unchanged.
[0054] Example 7
[0055] On the basis of Example 1, the mass ratio of the open hollow carbon to ammonium oxalate monohydrate and potassium bicarbonate in step (2) was changed to 1:2:4, and the other conditions remained unchanged.
[0056] Example 8
[0057] On the basis of Example 1, the mass ratio of the open hollow carbon to ammonium oxalate monohydrate and potassium bicarbonate in step (2) was changed to 1:6:4, and the other conditions remained unchanged.
[0058] Example 9
[0059] On the basis of Example 1, the mass ratio of the open hollow carbon to ammonium oxalate monohydrate and potassium bicarbonate in step (2) was changed to 1:8:4, and the other conditions remained unchanged.
[0060] Comparative Example 1
[0061] On the basis of Example 1, step (1) is not performed, and ordinary commercially available porous block activated carbon material is used instead of open hollow carbon, and other conditions remain unchanged.
[0062] Performance Characterization
[0063] (1) Catalytic activation of persulfate by the modified layered metal hydroxide composite catalyst material of the present invention
[0064] Prepare a simulated wastewater solution containing 10 mg / L DTZ, take 100 mL of simulated wastewater into the reactor, first add 0.03 g of potassium monopersulfate powder, then add 0.003 g of the catalytic materials prepared in Examples 1 to 9 and Comparative Example 1, respectively, stir at a magnetic stirring speed of 800 r / min, and react for 15 min. During the reaction, the concentration of DTZ was analyzed by high performance liquid chromatography. The test results are as follows: Figures 1-2 shown.
[0065] Depend on Figure 1 It can be obtained that the degradation rates of DTZ in 15min by activating persulfuric acid potassium monopersulfate in the catalytic materials of Examples 1 to 5 are 100%, 80%, 85%, 73%, and 69%, respectively. Example 1, that is, the catalytic material with a reaction time of 16h can achieve a 100% degradation effect in about 12min. When the reaction time is 8h, the reaction time is short at this time, and the opening requirement has not been met. Only a few carbon balls can be opened, and the active sites on the inner surface are not fully utilized, so the degradation effect is general; as the reaction time is extended, it reaches the best at 16h, at which time LDH can grow longitudinally on the inner and outer surfaces of the material, exposing more active sites; and when the reaction time is further increased, the degradation effect becomes worse, mainly because as the reaction time increases, the material thickness and neck length increase at this time, which reduces the active sites available for the same quality of material, and the longer neck structure hinders the growth of metal on its inner surface. Compared with Comparative Example 1, Examples 1 to 5 have achieved better catalytic effects.
[0066] Depend on Figure 2It can be obtained that the degradation rates of DTZ in 15 minutes by activating persulfate potassium monopersulfate in the catalytic materials of Examples 1 to 5 are 100%, 85%, 100%, 100%, and 100%, respectively. When the addition amount of ammonium oxalate monohydrate is 0, the addition amount of N is 0 at this time, and the degradation effect is general. After 15 minutes, the pollutants are still not completely degraded; as the addition amount of ammonium oxalate monohydrate increases, due to the different electronegativity of nitrogen and carbon, the charge distribution of carbon atoms will be significantly affected by the adjacent nitrogen dopant, and the graphite nitrogen N generated under high temperature conditions can promote the interaction between persulfate / organic matter and carbon material, thereby enhancing the adsorption capacity and catalytic activity of persulfate activation. In addition, the N-doped carbon plays a dual role of generating free radicals and preventing the leaching and aggregation of metal active centers, ensuring the continuous activation of the material. N-doped carbon usually exhibits lower oxidation resistance because the introduction of N atoms inevitably introduces defects into carbon materials. It is well known that the corrosion of carbon materials occurs faster at defect locations, so further increasing the amount of ammonium oxalate monohydrate does not increase the degradation effect of the material. When the amount of ammonium oxalate monohydrate added reaches a mass ratio of 1:2:4, the degradation rate is obviously accelerated in the first 15 minutes, and a 100% degradation effect is achieved at 15 minutes. With the further increase in the amount of ammonium oxalate monohydrate, when the mass ratio of the added amount is 1:4:4, the degradation effect is optimal. Not only is the degradation rate accelerated in the first 15 minutes, but a 100% degradation effect can be achieved in 12 minutes. Further increasing the amount of N doping, the promotion effect is not obvious at this time, so the mass ratio of 1:4:4 is selected as the best choice.
[0067] (2) System comparison experiment
[0068] In order to compare the excellent degradation effect of the materials, the modified layered metal hydroxide composite catalytic material was prepared by adding PMS alone, open hollow carbon (NHOC) alone, open hollow carbon (NHOC) + PMS, open hollow carbon (NHOC) + PMS + metal hydroxide, and Example 1 in the degradation experiment, and the degradation results of adding different materials were observed. The test results are as follows: Figure 3 shown.
[0069] Depend on Figure 3 It can be seen that PMS alone has basically no degradation effect on water bodies; the open carbon prepared in step (1) of Example 1 has only an adsorption effect on pollutants after being added alone; adding PMS while adding the open carbon material can find that the activation effect is general; the carbon material and LDH are prepared separately and mechanically mixed before being added, and the effect is improved; compared with the above four groups of experiments, the composite material prepared in Example 1 has a significant effect after being added to the simulated wastewater.
[0070] (3) Cycle test
[0071] In order to verify the stability of the composite catalytic material synthesized in the present invention, repeated experiments were conducted using the catalytic material prepared in Example 1, which was washed with ultrapure water after use and dried in a vacuum oven at 60°C before the next cycle. The test results are as follows: Figure 4 shown.
[0072] like Figure 4 As shown, the degradation effect of the catalytic material prepared in Example 1 on DTZ in four runs was investigated. The results show that the composite catalyst of the present invention has good stability during the degradation process and can still achieve a degradation rate of more than 95% within 15 minutes in the fourth cycle.
[0073] Structural characterization
[0074] Figure 5 The SEM and mapping images of the catalytic material prepared in Example 1 of the present invention. It can be seen from the figure that the unloaded open hollow carbon ( Figure 6 ) It can be clearly seen from the comparison that metal hydroxides grow on the surface of the material, and the mapping diagram also proves the presence of metal elements on the surface of the carbon material.
Claims
1. A modified layered metal hydroxide composite catalytic material, It is characterized in that The invention comprises a carrier open hollow carbon and a metal hydroxide loaded on the carrier, wherein the metal hydroxide grows vertically on the inner and outer surfaces of the open hollow carbon.
2. The modified layered metal hydroxide composite catalytic material according to claim 1, It is characterized in that The open hollow carbon is doped with nitrogen.
3. A method for preparing the modified layered metal hydroxide composite catalytic material according to claim 1 or 2, It is characterized in that The following steps are involved: (1) mixing the open hollow carbon with a nitrogen source and bicarbonate, and then calcining at a high temperature to obtain nitrogen-doped open hollow carbon; (2) dissolving the metal salt and urea in a solvent, adding nitrogen-doped open hollow carbon to obtain a suspension, and performing a solvent thermal synthesis reaction to obtain the layered metal hydroxide composite catalytic material.
4. The method for preparing the modified layered metal hydroxide composite catalytic material according to claim 3, It is characterized in that In step (1), the mass ratio of the open hollow carbon to the nitrogen source and the bicarbonate is 1:0:4 to 1:8:
4.
5. The method for preparing the modified layered metal hydroxide composite catalytic material according to claim 3, It is characterized in that In step (2), the solvent is ethanol, and the solvent thermal synthesis reaction temperature is 100-160°C.
6. The method for preparing the modified layered metal hydroxide composite catalytic material according to claim 3, It is characterized in that The preparation method of the open hollow carbon is as follows: premixing two soft templates of sodium dodecyl sulfate and block polyether P123, adding a carbon source, and then performing a hydrothermal carbonization reaction, and obtaining the open hollow carbon after the reaction is completed.
7. The method for preparing the modified layered metal hydroxide composite catalytic material according to claim 6, It is characterized in that The molar ratio of the sodium dodecyl sulfate to the block polyether P123 is 1:1-5.
8. The method for preparing the modified layered metal hydroxide composite catalytic material according to claim 6, It is characterized in that The temperature of the hydrothermal carbonization reaction is 150-200° C., and the time is 8-24 hours.
9. Use of the modified layered metal hydroxide composite catalytic material according to claim 1 or 2 in activating persulfate to degrade organic pollutants.
10. The use according to claim 9, It is characterized in that The organic pollutant is an iodinated X-ray contrast agent.