Method for recovering copper from waste PCB (printed circuit board) through enhanced flotation
By applying flotation technology and ultrasonic coupled shear strengthening technology in waste PCB, the problems of high energy consumption and hazardous waste in the existing technology are solved, and efficient and environmentally friendly copper recycling is achieved, which significantly improves the recovery rate and concentrate. purity.
Patent Information
- Application Number
- CN202410985930.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has high energy consumption, hazardous waste generation and safety risks in recycling valuable metals from waste PCBs, limiting its industrial applications.
Using flotation technology combined with ultrasonic coupled shear strengthening technology, copper is extracted from the waste PCB, and metal-containing powder is obtained by crushing and grinding, and added to the flotation machine for pre-stirring and flotation, and using collectors, activators and foaming agents. Separation, ultrasonic waves and shear flow fields are applied to improve the recovery efficiency and purity of copper.
It realizes efficient and environmentally friendly recycling of copper from waste PCB, reduces recycling costs, avoids the generation of harmful waste gas and wastewater, and significantly improves the copper recovery rate and the purity of concentrate.
Smart Images

Figure BDA0004957395100000031
Abstract
Description
Technical Field
[0001] The invention specifically relates to a method for recovering copper from waste PCBs by enhanced flotation, and belongs to the field of waste recycling. Background Art
[0002] Waste PCBs contain a large number of harmful elements and substances, such as mercury, lead, nickel, polybrominated biphenyls (PBB), polybrominated diphenyl ethers (PBDE), etc. If they are only treated by simple crushing, incineration or landfill, it will cause serious environmental pollution and damage, and seriously endanger human health. On the other hand, waste PCBs are "urban mine" resources containing precious metals such as gold, silver, platinum, and a large number of basic metals such as copper, iron, tin, and aluminum. Compared with ordinary ores, the metal grade of waste PCBs is dozens or even hundreds of times higher, and has a very high comprehensive recycling value. Recovering valuable metals from waste PCBs can realize the resource recycling of waste, protect the ecological environment, and greatly promote the process of sustainable development.
[0003] At present, physical and mechanical treatment, pyrometallurgy, hydrometallurgy and biometallurgy can be used to recover valuable metals from waste PCBs. Among them, pyrometallurgy and hydrometallurgy are the most widely used. The pyrometallurgical treatment method has the advantages of large processing capacity and strong adaptability of raw materials, but it will produce a large amount of harmful waste during the recovery process, which will also cause air pollution. In addition, high energy consumption and loss of valuable metals are also noteworthy disadvantages. The metal recovery rate and metal purity of the hydrometallurgical method are both high, but because strong acids, strong alkalis, halides, etc. are used as leaching agents during the treatment process, there are greater safety risks, which limits its large-scale industrial application. Therefore, it is urgent to develop more green, environmentally friendly, efficient and energy-saving valuable metal recovery and treatment technologies to achieve sustainable mining and utilization of waste PCBs in "urban mines". Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for recovering copper from waste PCBs by enhanced flotation. The method provided by the present invention can realize the efficient and environmentally friendly extraction of valuable metal copper from waste PCBs, greatly reduce the recovery cost of copper in waste PCBs, avoid the generation and emission of harmful waste gas in the traditional recovery process, and obtain copper-containing concentrate that is conducive to further recovery, so as to achieve the purpose of efficient and clean resource utilization of valuable metals in waste PCBs:
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for recovering copper from waste PCBs by enhanced flotation, wherein the waste PCBs are crushed and ground to obtain metal-containing powders, the metal-containing powders are added to the flotation tank of a flotation machine for pre-stirring to prepare slurry, and a collector is added according to a predetermined dosage and fully stirred until completely dissolved. The stirring speed and air flow are controlled, and the flotation process is carried out under the effect of ultrasonic coupling shear enhancement. After the flotation process is completed, flotation concentrates and tailings are obtained, and the tailings are returned for further flotation treatment.
[0007] In the method, more than 80% of the metal-containing powder particles obtained by crushing and grinding are smaller than 200 meshes.
[0008] In the method, the solid content of the slurry is 20% to 60%, the pre-stirring time is 2 to 10 minutes, and the stirring speed is 500 to 2000 rpm. Preferably, the solid content of the slurry is 20% to 50%, the pre-stirring time is 2 to 5 minutes, and the stirring speed is 800 to 1100 rpm.
[0009] In the method, the collector is a combination of two or more of sodium alkyl sulfonate, sodium alkyl sulfate, phosphate, arsenate, kerosene, oleic acid, stearic acid, and palmitic acid, and the addition amount is 1-10 kg / t; the activator is sulfuric acid or sodium hydroxide, which is used to adjust the pH of the system; the foaming agent is one of pine oil, cresol oil, isobutyl methyl benzyl alcohol, methyl amyl alcohol, pine oil, and diacetone alcohol oil, and the total addition amount is 0.05-0.8 kg / t. Preferably, the collector is a combination of oleic acid, stearic acid, and palmitic acid, the addition amount of oleic acid is 0.6-1.5 kg / t, the addition amount of stearic acid is 0.8-1.3 kg / t, and the addition amount of palmitic acid is 0.4-1.0 kg / t; the activator is sulfuric acid or sodium hydroxide, and the pH value of the system is adjusted to 5-8; the foaming agent is one of pine oil and diacetone alcohol oil, and the addition amount is 0.1-0.4 kg / t.
[0010] The method described above has a stirring rate of 1000-3500 rpm and an air flow rate of 0.1-0.4 m 3 Preferably, the stirring rate is 1000-2500 rpm and the air flow rate is 0.1-0.25 m 3 / h.
[0011] In the method, the ultrasonic frequency of ultrasonic coupling shear strengthening is 30-500kHz, the ultrasonic power is 10-300W, and the shear rate is 2000-10000rpm. Preferably, the ultrasonic frequency of ultrasonic coupling shear strengthening is 100-400kHz, the ultrasonic power is 100-250W, and the shear rate is 3000-6000rpm.
[0012] Principles and advantages
[0013] The method of the present invention innovatively introduces the flotation process used for mineral processing into the process of copper recovery from waste PCBs, and utilizes the different hydrophilicity of various metal-containing particles to separate copper-containing particles from other particles, thereby achieving efficient and selective separation and recovery of valuable metals. Compared with traditional pyrometallurgical and hydrometallurgical treatment processes, the flotation process has lower energy consumption and does not produce toxic waste gas and wastewater. In addition, the present invention also utilizes the ultrasonic coupling shear strengthening effect. On the one hand, the cavitation effect of ultrasonic waves can effectively strip organic matter and oxide inclusions on the surface of copper-containing particles, further improving the purity of copper-containing concentrates; on the other hand, the shear flow field is used to refine the bubbles, further reduce the volume of the slurry bubbles, increase the contact area between the bubbles and the slurry, and further improve the flotation efficiency. Therefore, based on the multi-physical field coupling strengthening effect of the ultrasonic field and the shear flow field, the flotation recovery efficiency of valuable metal copper in waste PCBs and the purity of copper-containing concentrates can be significantly improved.
[0014] The present invention aims to solve the problems of high cost, secondary pollution and high energy consumption of metal copper recovery in existing waste PCBs, and provides a method for recovering copper with high selectivity, high flotation efficiency and energy saving and environmental protection. The present invention is of great significance to promoting the technological progress of sustainable recycling of resources and energy saving and consumption reduction. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] none Specific implementation plan
[0016] The following examples are intended to further illustrate the present invention but are not intended to limit the present invention.
[0017] Example 1
[0018] The raw materials are waste PCBs provided by a company, and their main metal components and contents are as follows:
[0019]
[0020] The waste PCB is crushed and ground to obtain 200g of metal-containing powder, of which more than 80% of the powder particles are smaller than 200 mesh. The metal-containing powder is added to the flotation tank of the flotation machine and pre-stirred at 1000rpm for 3 minutes to prepare a slurry with a solid content of 30%. Flotation agents are added in the following proportions: collector oleic acid 1.2kg / t, stearic acid 1.1kg / t, palmitic acid 0.6kg / t; foaming agent pine oil 0.2kg / t, sulfuric acid or sodium hydroxide is used as an activator to adjust the pH to 5-8, and stir thoroughly until the flotation agent is completely dissolved. During the flotation process, the stirring speed is controlled at 2000rpm and the air flow rate is 0.15m 3 / h, and simultaneously applied ultrasonic coupling shearing intensification external field intensified flotation process with ultrasonic frequency of 200kHz, ultrasonic power of 100W and shear rate of 5000rpm. After the flotation process is completed, flotation concentrate and tailings are obtained, and the tailings are returned for further flotation treatment. The copper-containing concentrate is analyzed for composition, and the recovery rate of valuable metal copper in the waste PCB is calculated to be 98.95%.
[0021] Example 2
[0022] Use the waste PCB as shown in Example 1 as raw material, crush and grind the waste PCB to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are smaller than 200 mesh. Add the metal-containing powder to the flotation tank of the flotation machine, pre-stir for 4 minutes at 1100rpm to prepare a slurry with a solid content of 50%. Add flotation agents in the following proportions: collector oleic acid 0.9kg / t, stearic acid 1.3kg / t, palmitic acid 1.0kg / t; foaming agent diacetone alcohol oil 0.4kg / t, use sulfuric acid or sodium hydroxide as an activator to adjust the pH to 5-8, and stir thoroughly until the flotation agent is completely dissolved. During the flotation process, control the stirring speed to 1500rpm and the air flow to 0.25m 3 / h, and simultaneously applied ultrasonic coupling shearing intensification external field intensified flotation process with ultrasonic frequency of 300kHz, ultrasonic power of 200W and shear rate of 4000rpm. After the flotation process is completed, flotation concentrate and tailings are obtained, and the tailings are returned for further flotation treatment. The copper-containing concentrate is analyzed for composition, and the recovery rate of valuable metal copper in the waste PCB is calculated to be 99.26%.
[0023] Example 3
[0024] Use the waste PCB as shown in Example 1 as raw material, crush and grind the waste PCB to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are smaller than 200 mesh. Add the metal-containing powder to the flotation tank of the flotation machine, and pre-stir for 5 minutes at 800rpm to prepare a slurry with a solid content of 40%. Add flotation agents in the following proportions: collector oleic acid 1.1kg / t, stearic acid 1.2kg / t, palmitic acid 0.6kg / t; foaming agent pine oil 0.1kg / t, use sulfuric acid or sodium hydroxide as an activator to adjust the pH to 5-8, and stir thoroughly until the flotation agent is completely dissolved. During the flotation process, control the stirring speed to 2000rpm and the air flow to 0.15m 3 / h, and simultaneously applied ultrasonic coupling shearing intensification external field intensified flotation process with ultrasonic frequency of 200kHz, ultrasonic power of 100W and shear rate of 5000rpm. After the flotation process is completed, flotation concentrate and tailings are obtained, and the tailings are returned for further flotation treatment. The copper-containing concentrate is analyzed for composition, and the recovery rate of valuable metal copper in the waste PCB is calculated to be 97.51%.
[0025] Comparative Example 1 (no ultrasonic enhancement)
[0026] Use the waste PCB as shown in Example 1 as raw material, crush and grind the waste PCB to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are smaller than 200 mesh. Add the metal-containing powder to the flotation tank of the flotation machine, and pre-stir for 3 minutes at 1000rpm to prepare a slurry with a solid content of 30%. Add flotation agents in the following proportions: collector oleic acid 1.2kg / t, stearic acid 1.1kg / t, palmitic acid 0.6kg / t; foaming agent pine oil 0.2kg / t, use sulfuric acid or sodium hydroxide as an activator to adjust the pH to 5-8, and stir thoroughly until the flotation agent is completely dissolved. During the flotation process, control the stirring speed to 2000rpm and the air flow to 0.15m 3 / h, and a shear-enhanced external field flotation process with a shear rate of 5000rpm was applied. After the flotation process was completed, flotation concentrate and tailings were obtained, and the tailings were returned for further flotation treatment. The copper-containing concentrate was analyzed for composition, and the recovery rate of valuable metal copper in the waste PCB was calculated to be 91.26%.
[0027] Comparative Example 2 (without shear strengthening)
[0028] Use the waste PCB as shown in Example 1 as raw material, crush and grind the waste PCB to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are smaller than 200 mesh. Add the metal-containing powder to the flotation tank of the flotation machine, and pre-stir for 3 minutes at 1000rpm to prepare a slurry with a solid content of 30%. Add flotation agents in the following proportions: collector oleic acid 1.2kg / t, stearic acid 1.1kg / t, palmitic acid 0.6kg / t; foaming agent pine oil 0.2kg / t, use sulfuric acid or sodium hydroxide as an activator to adjust the pH to 5-8, and stir thoroughly until the flotation agent is completely dissolved. During the flotation process, control the stirring speed to 2000rpm and the air flow to 0.15m 3 / h, and simultaneously applied an ultrasonic enhanced external field enhanced flotation process with an ultrasonic frequency of 200kHz and an ultrasonic power of 100W. After the flotation process is completed, flotation concentrate and tailings are obtained, and the tailings are returned for further flotation treatment. The copper-containing concentrate is analyzed for composition, and the recovery rate of valuable metal copper in the waste PCB is calculated to be 79.61%.
[0029] Comparative Example 3 (without ultrasonic coupling shear strengthening)
[0030] Use the waste PCB as shown in Example 1 as raw material, crush and grind the waste PCB to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are smaller than 200 mesh. Add the metal-containing powder to the flotation tank of the flotation machine, and pre-stir for 3 minutes at 1000rpm to prepare a slurry with a solid content of 30%. Add flotation agents in the following proportions: collector oleic acid 1.2kg / t, stearic acid 1.1kg / t, palmitic acid 0.6kg / t; foaming agent pine oil 0.2kg / t, use sulfuric acid or sodium hydroxide as an activator to adjust the pH to 5-8, and stir thoroughly until the flotation agent is completely dissolved. During the flotation process, control the stirring speed to 2000rpm and the air flow to 0.15m 3 / h. After the flotation process is completed, flotation concentrate and tailings are obtained, and the tailings are returned for further flotation treatment. The copper-containing concentrate is analyzed for composition, and the recovery rate of valuable metal copper in the waste PCB is calculated to be 58.39%.
Claims
1. A method for recovering copper from waste PCBs by enhanced flotation, characterized in that: The waste PCB is crushed and ground to obtain metal-containing powder, which is added to the flotation tank of the flotation machine for pre-stirring to form a slurry, and the collector, activator, and frother are added according to the predetermined dosage and stirred until they are completely dissolved. The stirring speed and air flow are controlled, and the flotation process is carried out under the effect of ultrasonic coupling shear strengthening. After the flotation process is completed, flotation concentrate and tailings are obtained, and the tailings are returned for further flotation treatment.
2. The method according to claim 1, characterized in that: The metal-containing powder obtained by crushing and grinding has more than 80% of the powder particles smaller than 200 meshes.
3. The method according to claim 1, characterized in that: The solid content of the slurry is 20% to 60%, the pre-stirring time is 2 to 10 minutes, and the stirring speed is 500 to 2000 rpm.
4. The method according to claim 1, characterized in that: The collector is a combination of two or more of sodium alkyl sulfonate, sodium alkyl sulfate, phosphate, arsenate, kerosene, oleic acid, stearic acid, and palmitic acid, and the addition amount is 1-10 kg / t; the activator is sulfuric acid or sodium hydroxide, which is used to adjust the pH value of the system; the foaming agent is one of pine oil, cresol oil, isobutyl methyl benzyl alcohol, methyl amyl alcohol, pine oil, and diacetone alcohol oil, and the addition amount is 0.05-0.8 kg / t.
5. The method according to claim 1, characterized in that: The stirring rate is 1000-3500 rpm, and the air flow rate is 0.1-0.4 m 3 / h.
6. The method according to claim 1, characterized in that: The ultrasonic frequency of the ultrasonic coupling shear strengthening is 30-500kHz, the ultrasonic power is 10-300W, and the shear rate is 2000-10000rpm.
Citation Information
Patent Citations
Method for recovering pure copper from waste circuit board
CN108677021A
Powerful mixing and shearing device and method suitable for fine mineral flotation
CN114713382A
Circuit board recovery processing device
CN118268123A
Novel hyperacoustic flotation equipment of peripheral radiation
CN205308587U
Flotation machine
CN208928383U