Application of dolomite inhibitor polyepoxysuccinic acid in phosphate ore flotation magnesium removal
By using polyepoxysuccinic acid as an inhibitor in phosphate ore flotation, the problem of difficulty in separation between apatite and dolomite is solved, and low-cost and environmentally friendly separation is achieved Effects, simplify the process flow and reduce the magnesium content.
Patent Information
- Application Number
- CN202411099569.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to effectively separate apatite and dolomite, resulting in excess of the magnesium content in phosphorus concentrate, and the addition of commonly used inhibitors such as sulfuric acid or phosphoric acid is large, economical, and may cause environmental pollution and equipment corrosion.
Polyepoxysuccinic acid is used as a dolomite inhibitor, and selectively adsorbs the surface of dolomite minerals through its chelation and steric hindrance effects during the flotation process of phosphate ore, which weakens the adsorption of collectors and realizes phosphorus Effective separation of greystone and dolomite.
The effective separation of apatite and dolomite is achieved, the amount of collector is used, the risk of environmental pollution and equipment corrosion is reduced, and the process flow is simplified and the operation is convenient.
Smart Images

Figure CN118925941A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of phosphate rock flotation, and in particular relates to application of dolomite inhibitor polyepoxysuccinic acid in phosphate rock flotation and magnesium removal. Background Art
[0002] my country's phosphate resources are abundant but not rich, mostly in the form of medium and low-grade phosphate ore. The useful mineral apatite in this type of ore often coexists closely with gangue minerals such as dolomite, quartz, and calcite. Among them, dolomite and apatite minerals have the most similar surface properties and very similar floatability. It is difficult to achieve effective separation of the two using traditional fatty acid collectors, resulting in excessive magnesium content in phosphate concentrate, which seriously affects the efficient utilization of phosphorus resources. At present, sulfuric acid or phosphoric acid is often added as an inhibitor during the flotation process of phosphate ore to reduce the floatability of apatite, so as to achieve the separation of the two using the reverse flotation process. However, when sulfuric acid or phosphoric acid is used as an inhibitor, the amount of reagent added is usually large, the economy is poor, and it is easy to cause environmental pollution and equipment corrosion.
[0003] Therefore, how to provide a selective, low-cost, non-toxic and environmentally friendly apatite and dolomite separation inhibitor is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes the use of dolomite inhibitor polyepoxysuccinic acid in the flotation and magnesium removal of phosphate ore.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] Application of polyepoxysuccinic acid, a dolomite inhibitor, in the flotation and magnesium removal of phosphate ore.
[0007] A phosphate ore flotation and magnesium removal process comprises the process of crushing, grinding, slurry adjustment and flotation, wherein polyepoxysuccinic acid is added as an inhibitor during the slurry adjustment process.
[0008] Preferably, the concentration of the polyepoxysuccinic acid in the phosphate ore flotation slurry obtained after slurry adjustment is (50-80) mg / L.
[0009] Preferably, the polyepoxysuccinic acid is added in the form of a solution, and the mass concentration of the polyepoxysuccinic acid solution is 0.5-1%.
[0010] Beneficial effects: Polyepoxysuccinic acid (PESA) is a nitrogen-free, non-phosphorus organic compound with advantages such as good biodegradability and low price, and is widely used in the field of water treatment. PESA has a large number of carboxyl groups, which can strongly chelate with metal ions such as calcium and magnesium and adsorb on the surface of minerals, thereby increasing their surface hydrophilicity. In addition, due to the large cross-sectional size of the PEAS polar group, it can increase its steric hindrance effect when interacting with the mineral surface, improve its selectivity on the mineral surface, and be more conducive to the separation of minerals with similar surface active site atoms. At the same time, the pre-adsorption of PESA can also reduce the number of exposed active sites on the mineral surface, weaken the adsorption effect of the collector, and achieve mineral flotation inhibition. The polyepoxysuccinic acid in the present invention can selectively adsorb on the surface of dolomite minerals under the synergistic effect of chelation and steric hindrance effect, but not adsorb or weakly adsorb on the surface of apatite minerals, thereby significantly reducing the adsorption of the collector sodium oleate on the dolomite surface without affecting the adsorption of sodium oleate on the apatite surface, thereby enhancing the difference in floatability between dolomite and apatite and achieving effective separation of the two.
[0011] Preferably, the pH value of the phosphate ore flotation slurry obtained after the slurry adjustment is 6.5 to 8.5.
[0012] Beneficial effects: When PESA is used as a depressant, the optimal flotation pH value is 6.5-8.5. Within this pH range, the surface dissolution of phosphate ore is small, and the reagent consumption is small. At the same time, within this pH range, the slurry has weak corrosion on the equipment, which can extend the service life of the equipment.
[0013] Preferably, sodium oleate is added as a collector during the flotation process.
[0014] Preferably, the ratio of the amount of sodium oleate added to the phosphate rock flotation slurry obtained after slurry adjustment is (60-100) mg:1L.
[0015] Preferably, the sodium oleate is added in the form of a solution, and the mass concentration of the sodium oleate solution is 1-4%.
[0016] Preferably, the crushing is to crush the phosphate ore into particles with a size of less than 2 mm.
[0017] Preferably, the grinding is to mix the ore particles obtained after crushing with water to obtain a grinding slurry with a mass concentration of 40% to 60%, and then use wet grinding to grind the ore until the content of particles with a particle size of less than 74 μm accounts for 70% to 85%.
[0018] Beneficial effect: The selection of grinding particle size is based on the embedded particle size of useful minerals in phosphate ore. When most of the phosphate ores in my country are finely ground to -74μm and the content accounts for 70% to 85%, the monomer dissociation of most useful minerals (apatite) can be achieved.
[0019] Compared with the prior art, the present invention has the following advantages and technical effects:
[0020] Compared with the commonly used industrial phosphate rock demagnesium removal inhibitors, the dolomite inhibitor polyepoxysuccinic acid provided by the present invention has the advantages of small dosage, strong selectivity, good inhibition effect, small environmental pollution, and lax flotation conditions. At the same time, the inhibitor can be used to achieve direct flotation demagnesiumization of phosphate rock. Compared with the existing direct-reverse flotation combined process, the direct flotation demagnesiumization provided by the present invention can be combined with direct flotation desiliconization, which has the advantages of short process flow, convenient operation, easy treatment of tailings, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0022] Figure 1 The present invention provides a process flow chart for the flotation and demagnesization of phosphate rock. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0025] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources;
[0026] The phosphate rock used in the embodiment of the present invention is actually taken from a place in Guizhou. After chemical multi-element analysis, it is known that its main components are calculated by mass percentage: 2 O 5 :28.38%, CaO:53.72%, Al 2 O 3 :3.65%, F:3.25%, SiO 2 :1.58%, MgO:3.53%, and the rest are impurities;
[0027] The inhibitor polyepoxysuccinic acid (PESA) and the collector sodium oleate used in the embodiments of the present invention are both industrially pure, and the pH adjusters sodium hydroxide and hydrochloric acid are both chemically pure.
[0028] The process flow chart of phosphate rock flotation demagnesization provided in Examples 1-4 of the present invention is as follows Figure 1 shown.
[0029] In the phosphate concentrate product obtained by flotation in the embodiment of the present invention, P 2 O 5 The grade is calculated as follows:
[0030] The calculation method of MgO grade is:
[0031] The calculation method of phosphorus recovery is:
[0032] Where, ξ is the phosphorus recovery rate in concentrate, %; m 精 、m 原 are the mass of concentrate and ore, g; α 精 , α 原 P in concentrate and raw ore respectively 2 O 5 grade.
[0033] Example 1
[0034] Application of dolomite inhibitor polyepoxysuccinic acid in phosphate rock flotation and magnesium removal specifically comprises the following steps:
[0035] (1) Crushing and grinding: The phosphate ore is crushed by a disc crusher to a particle size of less than 2 mm, and then mixed with tap water to form a grinding slurry with a mass concentration of 40%. The slurry is then wet-ground by a ball mill until the content of particles with a particle size of less than 74 μm accounts for 70%, thereby obtaining a finely ground slurry.
[0036] (2) Slurry adjustment: The finely ground pulp is placed in an aerated hanging tank flotation machine, tap water and a 0.5% PESA solution as an inhibitor are added, and the pH is adjusted with a pH adjuster, and then stirred for 3 minutes at an impeller speed of 1700 rpm to obtain a phosphate rock flotation pulp; wherein the mass concentration of the flotation pulp is 15%, the pH adjuster is a 0.5% sodium hydroxide solution and / or a 0.5% hydrochloric acid dilute solution, and the pH value of the pulp is adjusted to 8.0, and the mass concentration of the PESA inhibitor in the phosphate rock flotation pulp is 50 mg / L.
[0037] (3) Flotation: At room temperature (22-25°C), add a 1% sodium oleate solution as a collector to the phosphate rock flotation slurry after slurry adjustment, wherein the amount of sodium oleate added is 60 mg / L based on the volume of the phosphate rock flotation slurry; after stirring for 3 minutes, open the aeration valve, control the aeration volume to 1 L / min, start the aeration flotation frothing operation, and the frothing time is 4 minutes. After the flotation is completed, the flotation froth product (concentrate product) and the product in the tank (tailings product) are dried, weighed, and tested for grade, and the product indicators are calculated.
[0038] In this embodiment, the phosphorus concentrate product obtained by flotation has P 2 O 5 The grade is 36.5%, the MgO grade is 1.4%, and the phosphorus recovery rate is 75.0%.
[0039] Example 2
[0040] Application of dolomite inhibitor polyepoxysuccinic acid in phosphate rock flotation and magnesium removal specifically comprises the following steps:
[0041] (1) Crushing and grinding: The phosphate ore is crushed by a disc crusher to a particle size of less than 2 mm, and then mixed with tap water to form a grinding slurry with a mass concentration of 50%. The slurry is then wet-ground by a ball mill until the content of particles with a particle size of less than 74 μm accounts for 75%, thereby obtaining a finely ground slurry.
[0042] (2) Slurry adjustment: The finely ground pulp is placed in an aerated hanging tank flotation machine, tap water and a 0.7% PESA inhibitor solution are added, and the pH is adjusted with a pH adjuster. The mixture is stirred for 3 minutes at an impeller speed of 1900 rpm to obtain a phosphate rock flotation pulp; wherein the mass concentration of the flotation pulp is 20%, the pH adjuster is a 0.7% sodium hydroxide solution and / or a 0.7% hydrochloric acid dilute solution, and the pH value of the pulp is adjusted to 6.5. The mass concentration of the PESA inhibitor in the phosphate rock flotation pulp is 70 mg / L.
[0043] (3) Flotation: At room temperature (22-25°C), add a 3% sodium oleate solution as a collector to the phosphate rock flotation slurry after slurry adjustment, wherein the amount of sodium oleate added is 80 mg / L based on the volume of the phosphate rock flotation slurry; after stirring for 4 minutes, open the aeration valve, control the aeration volume to 1.3 L / min, start the aeration flotation frothing operation, and the frothing time is 4 minutes. After the flotation is completed, the flotation froth product (concentrate product) and the product in the tank (tailings product) are dried, weighed, and tested for grade, and the product indicators are calculated.
[0044] In this embodiment, the phosphorus concentrate product obtained by flotation has P 2 O 5The grade is 36.9%, the MgO grade is 1.1%, and the phosphorus recovery rate is 81.3%.
[0045] Example 3
[0046] Application of dolomite inhibitor polyepoxysuccinic acid in phosphate rock flotation and magnesium removal specifically comprises the following steps:
[0047] (1) Crushing and grinding: The phosphate ore is crushed by a disc crusher to a particle size of less than 2 mm, and then mixed with tap water to form a slurry with a mass concentration of 60%. The slurry is then wet-ground by a ball mill until the content of particles with a particle size of less than 74 μm accounts for 85%, thereby obtaining a finely ground slurry.
[0048] (2) Slurry adjustment: The finely ground pulp is placed in an aerated hanging tank flotation machine, tap water and a PESA solution with a mass concentration of 1% are added, and the pH is adjusted with a pH adjuster, and then stirred for 3 minutes at an impeller speed of 2000 rpm to obtain a phosphate rock flotation pulp; wherein the mass concentration of the flotation pulp is 30%, the pH adjuster is a sodium hydroxide solution with a mass concentration of 1% and / or a dilute hydrochloric acid solution with a mass concentration of 1%, and the pH value of the pulp is adjusted to 8.5, and the mass concentration of the PESA inhibitor in the phosphate rock flotation pulp is 80 mg / L.
[0049] (3) Flotation: At room temperature (22-25°C), add a 4% sodium oleate solution as a collector to the phosphate rock flotation slurry after slurry adjustment, wherein the amount of sodium oleate added is 100 mg / L based on the volume of the phosphate rock flotation slurry; after stirring for 3 minutes, open the aeration valve, control the aeration volume to 1.5 L / min, start the aeration flotation frothing operation, and the frothing time is 5 minutes. After the flotation is completed, the flotation froth product (concentrate product) and the product in the tank (tailings product) are dried, weighed, and tested for grade, and the product indicators are calculated.
[0050] In this embodiment, the phosphorus concentrate product obtained by flotation has a content of P 2 O 5 The grade is 37.5%, the MgO grade is 0.92%, and the phosphorus recovery rate is 82.0%.
[0051] Example 4
[0052] Application of dolomite inhibitor polyepoxysuccinic acid in phosphate rock flotation and magnesium removal specifically comprises the following steps:
[0053] (1) Crushing and grinding: The phosphate ore is crushed by a disc crusher to a particle size of less than 2 mm, and then mixed with tap water to form a slurry with a mass concentration of 50%. The slurry is then wet-ground by a ball mill until the content of particles with a particle size of less than 74 μm accounts for 80%, thereby obtaining a finely ground slurry.
[0054] (2) Slurry adjustment: The finely ground slurry is placed in an aerated hanging tank flotation machine, tap water and a 0.5% PESA solution as an inhibitor are added, and the pH is adjusted with a pH adjuster, and then stirred for 3 minutes at an impeller speed of 1900 rpm to obtain a phosphate rock flotation slurry; wherein the mass concentration of the flotation slurry is 30%, the pH adjuster is a 0.5% sodium hydroxide solution and / or a 0.5% hydrochloric acid dilute solution, and the pH value of the slurry is adjusted to 7.5, and the mass concentration of the PESA inhibitor in the phosphate rock flotation slurry is 65 mg / L.
[0055] (3) Flotation: At room temperature (22-25°C), add a 2% sodium oleate solution as a collector to the phosphate rock flotation slurry after slurry adjustment, wherein the amount of sodium oleate added is 100 mg / L based on the volume of the phosphate rock flotation slurry; after stirring for 3 minutes, open the aeration valve, control the aeration volume to 1 L / min, start the aeration flotation frothing operation, and the frothing time is 5 minutes. After the flotation is completed, the flotation froth product (concentrate product) and the product in the tank (tailings product) are dried, weighed, and tested for grade, and the product indicators are calculated.
[0056] In this embodiment, the phosphorus concentrate product obtained by flotation has P 2 O 5 The grade is 37.0%, the MgO grade is 1.1%, and the phosphorus recovery rate is 85.0%.
[0057] Comparative Example 1
[0058] The invention discloses an application of polyepoxysuccinic acid as a dolomite inhibitor in the flotation removal of phosphate rock, which is different from the embodiment 1 in that an equal amount of sodium poly(acrylic acid-comaleic acid) is used in step (2) to replace PESA in the embodiment 1 as an inhibitor. The other process steps and parameters are the same as those in the embodiment 1.
[0059] In this embodiment, the phosphorus concentrate product obtained by flotation has P 2 O 5 The grade is 28.7%, the MgO grade is 2.11%, and the phosphorus recovery rate is 69.8%.
[0060] Comparative Example 2
[0061] The invention discloses an application of polyepoxysuccinic acid as a dolomite inhibitor in the flotation removal of phosphate rock, which is different from the embodiment 1 in that an equal amount of oxidized paraffin soap is used in step (3) to replace the sodium oleate in the embodiment 1 as a collector. The other process steps and parameters are the same as those in the embodiment 1.
[0062] In this embodiment, the phosphorus concentrate product obtained by flotation has P 2 O 5The grade is 30.2%, the MgO grade is 1.85%, and the phosphorus recovery rate is 72.3%.
[0063] Comparative Example 3
[0064] The invention discloses an application of dolomite inhibitor polyepoxysuccinic acid in phosphate rock flotation demagnesization, which is different from the embodiment 1 in that the mass concentration of the inhibitor PESA in the phosphate rock flotation slurry in step (2) is 30 mg / L. The other process steps and parameters are the same as those in the embodiment 1.
[0065] In this embodiment, the phosphorus concentrate product obtained by flotation has P 2 O 5 The grade is 31.5%, the MgO grade is 1.61%, and the phosphorus recovery rate is 83.2%.
[0066] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. Application of dolomite inhibitor polyepoxysuccinic acid in the flotation and magnesium removal of phosphate ore.
2. A phosphate ore flotation demagnesium process, including the process of crushing, grinding, slurry adjustment and flotation, characterized in that: Polyepoxysuccinic acid is added as an inhibitor during the slurry adjustment process.
3. A phosphate rock flotation demagnesium process according to claim 2, characterized in that: The concentration of the polyepoxysuccinic acid in the phosphate ore flotation slurry obtained after slurry adjustment is (50-80) mg / L.
4. A phosphate rock flotation demagnesium process according to claim 3, characterized in that: The polyepoxysuccinic acid is added in the form of a solution, and the mass concentration of the polyepoxysuccinic acid solution is 0.5-1%.
5. A phosphate rock flotation demagnesium process according to any one of claims 2 to 4, characterized in that: The pH value of the phosphate ore flotation slurry obtained after the slurry adjustment is 6.5-8.
5.
6. A phosphate rock flotation demagnesium process according to claim 2, characterized in that: Sodium oleate is added as a collector during the flotation process.
7. A phosphate rock flotation demagnesium process according to claim 6, characterized in that: The ratio of the amount of sodium oleate added to the phosphate rock flotation slurry obtained after slurry adjustment is (60-100) mg:1L.
8. A phosphate rock flotation demagnesium process according to claim 7, characterized in that: The sodium oleate is added in the form of a solution, and the mass concentration of the sodium oleate solution is 1-4%.
9. A phosphate rock flotation demagnesium process according to claim 2, characterized in that: The crushing is to crush the phosphate rock into particles with a size of less than 2 mm.
10. A phosphate rock flotation demagnesium process according to claim 2, characterized in that: The grinding is to mix the ore particles obtained after crushing with water to obtain a grinding slurry with a mass concentration of 40% to 60%, and then use wet grinding to grind the particles with a particle size less than 74 μm to account for 70% to 85%.
Citation Information
Patent Citations
Treatment method of iron separation tailings and application of polyepoxysuccinic acid
CN115350807A
Methods of controlling scale formation in the presence of metal ions in aqueous systems
US5468393A