Gradient different-temperature three-roller skew rolling equipment and preparation method of seamless metal composite pipe
Gradient heat of the inner and outer layers of seamless metal composite tubes is gradiently heated through the gradient differential temperature three-roll oblique rolling equipment, which solves the problem of brittle compounds in the bonding interface caused by high-temperature rolling and improves the combination of seamless metal composite tubes Strength and surface quality.
Patent Information
- Application Number
- CN202411007798.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-25
AI Technical Summary
In the prior art, when rolling metal seamless composite pipes with large performance differences such as steel/titanium, titanium/aluminum, steel/aluminum, etc., high-temperature rolling leads to the formation of brittle compounds at the bonding interface, reducing the binding strength, and seamless metal in the inner layer. The shapeability and oxidation resistance of the tubes are deteriorated, resulting in uneven wall thickness and poor surface quality.
Gradient temperature three-roll inclined rolling equipment is adopted to heat the inner and outer layers of seamless metal composite pipes separately, so that the outer seamless metal pipes maintain a high temperature during rolling, while the inner seamless metal pipe temperature is Below the outer layer, avoid the formation of brittle compounds, improve interface binding strength, and reduce deformation inconsistency.
It effectively improves the interface bonding strength of seamless metal composite pipes, improves wall thickness uniformity and surface quality, reduces the rolling force requirement, and extends the service life of rolls and mills.
Smart Images

Figure CN118926327A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of seamless metal composite pipe preparation, and in particular to a gradient different-temperature three-roller cross-rolling device and a method for preparing a seamless metal composite pipe. Background Art
[0002] At present, the preparation methods of seamless metal composite pipes mainly include explosion composite method, hydraulic composite method, drawing composite method and hot rolling composite method. The explosion composite method can realize one-time composite forming, and the prepared seamless metal composite pipe has high bonding strength; however, the explosion composite method has the disadvantages of low yield, poor uniformity of the formed seamless metal composite pipe, environmental pollution, and inability to achieve continuous forming. The hydraulic composite method and the drawing composite method have simple processes, but the bonding interface of the prepared seamless metal composite pipe is mechanical meshing, the bonding strength is low and there is a gap at the bonding interface. Once the liquid flows into the gap at the bonding interface, it will accelerate the corrosion of the seamless metal composite pipe and fail prematurely. The hot rolling composite method has the advantages of high production efficiency, low pollution, low energy consumption, and good product quality. It can also realize continuous forming along the axis and produce seamless metal composite pipes with a large aspect ratio. It is currently one of the most suitable methods for industrial production applications.
[0003] However, for seamless metal composite tubes such as steel / titanium, titanium / aluminum, steel / aluminum, titanium / copper, etc., which are formed by two metals with large differences in performance, the outer seamless metal tube has a higher deformation resistance, and a higher temperature is required for rolling forming. However, high-temperature rolling will cause a large amount of brittle compounds to be produced at the bonding interface and lead to a decrease in bonding strength. In addition, the formability and oxidation resistance of the inner seamless metal tube will deteriorate rapidly at high temperatures, resulting in uneven wall thickness and poor surface quality of the prepared metal composite tube, affecting subsequent use.
[0004] Therefore, lowering the rolling temperature can effectively inhibit the formation of brittle compounds at the bonding interface and improve the interface bonding strength. However, lowering the rolling temperature requires the rolling mill to have a higher rolling force, thereby increasing the wear and damage rate of the rolls and the rolling mill. In addition, when rolling at the same temperature, the inner and outer seamless metal tubes will have serious deformation inconsistencies, thereby reducing the interface bonding strength and increasing the head and tail removal amount, reducing the yield rate. Therefore, it is difficult to roll high-quality seamless metal composite tubes at the same temperature. Summary of the invention
[0005] The purpose of the present invention is to propose a gradient temperature-different three-roller cross-rolling equipment and a method for preparing a seamless metal composite pipe, which are used to improve the deformation coordination of metals with large performance differences, improve the interface bonding strength of the seamless metal composite pipe, and improve the uneven wall thickness and poor surface quality of the seamless metal composite pipe.
[0006] In order to achieve the above-mentioned purpose, in the first aspect, the present invention provides a gradient temperature-different three-roller cross-rolling equipment, comprising a first conveying mechanism, a first heating mechanism, a second conveying mechanism, a transfer mechanism, an ultrasonic induction heating mechanism, a three-roller cross-rolling mechanism and a first driving mechanism, wherein the first conveying mechanism is used to carry a seamless metal composite tube blank. The first conveying mechanism is also used to drive the seamless metal composite tube blank through the heating zone of the first heating mechanism, and the first heating mechanism is used to heat both the inner seamless metal tube and the outer seamless metal tube of the seamless metal composite tube blank to a first temperature. The second conveying mechanism is used to carry the seamless metal composite tube blank heated by the first heating mechanism. The transfer mechanism is used to receive the seamless metal composite tube blank heated by the first heating mechanism and transfer the seamless metal composite tube blank to the bearing surface of the second conveying mechanism. The ultrasonic induction heating mechanism is used to heat the outer seamless metal tube of the seamless metal composite tube blank heated by the first heating mechanism to a second temperature, and the inner seamless metal tube of the seamless metal composite tube blank is heated to a third temperature by heat conduction of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, and the third temperature is greater than or equal to the first temperature. The three-roller cross-rolling mechanism is used to roll the seamless metal composite tube billet heated by the ultrasonic induction heating mechanism. The first driving mechanism is used to drive the seamless metal composite tube billet on the second conveying mechanism to pass through the heating zone of the ultrasonic induction heating mechanism and enter the three-roller cross-rolling mechanism.
[0007] When the above technical solution is adopted, the first conveying mechanism can drive the seamless metal composite tube billet to pass through the heating zone of the first heating mechanism, so that the inner seamless metal tube and the outer seamless metal tube of the seamless metal composite tube billet are heated to the first temperature as a whole, and at this time, the temperature of the inner seamless metal tube and the outer seamless metal tube are the same. Afterwards, the transfer mechanism transfers the seamless metal composite tube billet heated by the first heating mechanism from the first conveying mechanism to the second conveying mechanism, and then, the first driving mechanism drives the seamless metal composite tube billet to pass through the heating zone of the ultrasonic induction heating mechanism to heat the outer seamless metal tube of the seamless metal composite tube billet, so that the temperature of the outer seamless metal tube is further increased and then enters the three-roller cross rolling mechanism for rolling. In this way, the outer seamless metal tube is heated to the second temperature, and the inner seamless metal tube of the seamless metal composite tube blank is heated to the third temperature by the heat conduction of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, and the third temperature is greater than or equal to the first temperature, which indicates that the temperature of the inner seamless metal tube is lower than the temperature of the bonding interface between the outer seamless metal tube and the inner seamless metal tube, and at the same time, the temperature of the bonding interface is lower than the temperature of the outer seamless metal tube, forming a seamless metal composite tube blank with a gradient temperature of the outer seamless metal tube-bonding interface-inner seamless metal tube. In this case, it is ensured that the outer seamless metal tube with higher deformation resistance has a higher temperature during rolling, and the temperature of the inner seamless metal tube is not too high, which effectively inhibits the generation of brittle compounds at the bonding interface and improves the interface bonding strength of the seamless metal composite tube. At the same time, it avoids the inner seamless metal tube from being too high in temperature, which leads to poor formability and oxidation resistance of the inner seamless metal tube, and improves the uneven wall thickness and poor surface quality of the seamless metal composite tube. In addition, during rolling, the outer seamless metal tube-bonding interface-inner seamless metal tube has a gradient temperature, which reduces the serious deformation incoordination of the inner and outer seamless metal tubes, thereby effectively improving the interface bonding strength and reducing the head and tail cutting amount, thereby improving the yield rate. Furthermore, there is no need to reduce the rolling temperature, avoiding the need for a higher rolling force during rolling, which exceeds the maximum rolling capacity that the three-roller inclined rolling mill can provide, resulting in rolling jams, ensuring the forming quality of the seamless metal composite tube, reducing the wear of the rollers and the three-roller inclined rolling mill, and slowing down the damage rate.
[0008] In a second aspect, the present invention provides a method for preparing a seamless metal composite pipe. Based on the gradient temperature-differential three-roller cross-rolling equipment described in the first aspect, the method for preparing the seamless metal composite pipe comprises:
[0009] A seamless metal composite tube blank is provided, wherein the seamless metal composite tube blank comprises an inner seamless metal tube and an outer seamless metal tube which are coaxially sleeved;
[0010] Heating the seamless metal composite tube blank so that both the inner seamless metal tube and the outer seamless metal tube are heated to a first temperature;
[0011] The outer seamless metal tube of the seamless metal composite tube blank is subjected to ultrasonic induction heating, so that the outer seamless metal tube is heated to a second temperature, and the inner seamless metal tube is heated to a third temperature by heat conduction of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, the third temperature is greater than or equal to the first temperature, and the bonding interface temperature of the outer seamless metal tube and the inner seamless metal tube is between the third temperature and the second temperature;
[0012] The seamless metal composite tube billet is rolled to obtain a seamless metal composite tube.
[0013] When the above technical solution is adopted, the seamless metal composite tube blank is heated so that the inner seamless metal tube and the outer seamless metal tube of the seamless metal composite tube blank are both heated to the first temperature, and then the outer seamless metal tube of the seamless metal composite tube blank is subjected to ultrasonic induction heating, the outer seamless metal tube is heated to the second temperature, and the inner seamless metal tube of the seamless metal composite tube blank is heated to the third temperature by heat conduction heating of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, the third temperature is greater than or equal to the first temperature, and the temperature of the bonding interface between the outer seamless metal tube and the inner seamless metal tube is between the third temperature and the second temperature. This indicates that the temperature of the inner seamless metal tube is lower than the temperature of the bonding interface, and at the same time, the temperature of the bonding interface is lower than the temperature of the outer seamless metal tube, forming a seamless metal composite tube blank with a gradient temperature of the outer seamless metal tube-bonding interface-inner seamless metal tube. In this case, it is ensured that the outer seamless metal tube with high deformation resistance has a high temperature during rolling, and the temperature of the inner seamless metal tube is not too high, which effectively inhibits the formation of brittle compounds at the bonding interface and improves the interface bonding strength of the seamless metal composite tube. At the same time, it avoids the inner seamless metal tube from being too high in temperature, which leads to the deterioration of the formability and oxidation resistance of the inner seamless metal tube, and improves the uneven wall thickness and poor surface quality of the seamless metal composite tube. In addition, during rolling, the outer seamless metal tube-bonding interface-inner seamless metal tube has a gradient temperature, which reduces the serious deformation incoordination of the inner and outer seamless metal tubes, thereby effectively improving the interface bonding strength and reducing the head and tail cutting amount, and improving the yield rate. Furthermore, there is no need to reduce the rolling temperature to avoid the need for a higher rolling force during rolling, which exceeds the maximum rolling capacity that the three-roller inclined rolling mill can provide, resulting in rolling jams, ensuring the forming quality of the seamless metal composite tube, reducing the wear of the rollers and the three-roller inclined rolling mill, and slowing down the damage rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0015] Figure 1 A schematic structural diagram of a gradient temperature-differential three-roller cross-rolling device provided in an embodiment of the present invention;
[0016] Figure 2 Schematic diagram of the local structure of the gradient temperature-different three-roller cross-rolling equipment provided in the embodiment of the present invention Figure 1 ;
[0017] Figure 3 Schematic diagram of the local structure of the gradient temperature-different three-roller cross-rolling equipment provided in the embodiment of the present invention Figure 2 ;
[0018] Figure 4 Schematic diagram of the local structure of the gradient temperature-different three-roller cross-rolling equipment provided in the embodiment of the present invention Figure 3 ;
[0019] Figure 5 A schematic diagram of a partial structure of a first conveying mechanism provided in an embodiment of the present invention;
[0020] Figure 6 A schematic diagram of the structure of an ultrasonic induction heating mechanism provided by an embodiment of the present invention;
[0021] Figure 7 A schematic diagram of the structure of a cooling mechanism provided by an embodiment of the present invention;
[0022] Figure 8 A step diagram of a method for preparing a seamless metal composite pipe provided by an embodiment of the present invention;
[0023] Fig. 9 A schematic diagram of the interface between a TA2 tube and a 304 stainless steel tube formed by the method for preparing a seamless metal composite tube provided by the prior art;
[0024] Fig.10 It is a schematic diagram of the bonding interface between a TA2 tube and a 304 stainless steel tube formed by the method for preparing a seamless metal composite tube provided by an embodiment of the present invention.
[0025] Reference numerals:
[0026] 1-first conveying mechanism, 11-first lifting frame, 12-first rotating roller, 121-recessed portion,
[0027] 13-first sprocket, 14-first drive motor, 15-second sprocket, 16-first chain, 17-second chain,
[0028] 2-first heating mechanism, 3-second conveying mechanism, 31-second frame, 32-second driving motor,
[0029] 33-third sprocket, 34-fourth sprocket, 35-third chain, 36-V-type bracket, 4-transfer mechanism,
[0030] 41-first frame, 42-carrying frame, 43-turning frame, 44-inclined plate, 5-supersonic frequency induction heating mechanism, 6-three-roller oblique rolling mechanism, 7-first driving mechanism, 71-chain driving structure, 72-third frame, 73-core rod, 8-cooling mechanism, 81-mounting frame, 82-liquid inlet, 83-liquid outlet. DETAILED DESCRIPTION
[0031] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0033] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.
[0034] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0035] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0036] At present, when seamless metal composite pipes are rolled using the hot rolling composite method, for seamless metal composite pipes formed by two metals with large differences in performance such as steel / titanium, titanium / aluminum, steel / aluminum, titanium / copper, etc., since the outer seamless metal pipe has a high deformation resistance, rolling forming requires a higher temperature, but high-temperature rolling will cause a large amount of brittle compounds to be produced at the bonding interface and lead to a decrease in bonding strength, and the formability and oxidation resistance of the inner seamless metal pipe will rapidly deteriorate at high temperatures, resulting in uneven wall thickness and poor surface quality of the obtained seamless metal composite pipe, affecting subsequent use. Therefore, lowering the rolling temperature can effectively inhibit the generation of brittle compounds at the bonding interface and improve the interface bonding strength. However, lowering the rolling temperature requires the rolling mill to have a higher rolling force, thereby increasing the wear and damage rate of the rollers and the rolling mill. In addition, when rolling at the same temperature, the inner and outer seamless metal pipes will have serious deformation incoordination, resulting in the interface being subjected to more shear force, which may rub the already bonded area apart and cause the bonding interface to fail. At the same time, the softer inner seamless metal tube will bear more deformation during the rolling process and come out of the head and tail of the outer seamless metal tube, increasing the amount of cutting of the finished tube head and tail and increasing the loss. Therefore, it is difficult to roll high-quality seamless metal composite tubes at the same temperature.
[0037] Taking steel / titanium seamless metal composite tube as an example, when the steel / titanium seamless metal composite tube is prepared by hot rolling composite method, the seamless titanium tube and the seamless steel tube produce plastic deformation at high temperature, thereby realizing the interface metallurgical bonding. However, since the rolling temperature range of steel is generally 900℃-1200℃, and once the rolling temperature exceeds the phase transition temperature of titanium (the phase transition temperature of pure titanium is 882℃), titanium transforms from the close-packed hexagonal α phase to the body-centered cubic β phase. Since both β-phase titanium and steel are cubic crystal systems, brittle compounds such as Fe-Ti are easily generated at the interface between the seamless titanium tube and the seamless steel tube, reducing the interface bonding strength.
[0038] In order to solve the technical problems existing in the above-mentioned prior art, see Figures 1 to 4As shown, an embodiment of the present invention provides a gradient temperature-different three-roller cross-rolling device, comprising a first conveying mechanism 1, a first heating mechanism 2, a second conveying mechanism 3, a transfer mechanism 4, an ultrasonic induction heating mechanism 5, a three-roller cross-rolling mechanism 6 and a first driving mechanism 7, wherein the first conveying mechanism 1 is used to carry a seamless metal composite tube blank. The first conveying mechanism 1 is also used to drive the seamless metal composite tube blank through the heating zone of the first heating mechanism 2, and the first heating mechanism is used to heat both the inner seamless metal tube and the outer seamless metal tube of the seamless metal composite tube blank to a first temperature. The second conveying mechanism 3 is used to carry the seamless metal composite tube blank heated by the first heating mechanism 2. The transfer mechanism 4 is used to receive the seamless metal composite tube blank heated by the first heating mechanism 2, and transfer the seamless metal composite tube blank to the bearing surface of the second conveying mechanism 3. The ultrasonic induction heating mechanism 5 is used to heat the outer seamless metal tube of the seamless metal composite tube blank heated by the first heating mechanism to a second temperature, and the inner seamless metal tube of the seamless metal composite tube blank is heated to a third temperature by heat conduction of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, and the third temperature is greater than or equal to the first temperature. The three-roller cross-rolling mechanism 6 is used to roll the seamless metal composite tube billet heated by the ultrasonic induction heating mechanism. The first driving mechanism 7 is used to drive the seamless metal composite tube billet on the second conveying mechanism 3 to pass through the heating zone of the ultrasonic induction heating mechanism 5 and enter the three-roller cross-rolling mechanism 6.
[0039] When the above technical solution is adopted, the first conveying mechanism 1 can drive the seamless metal composite tube billet to pass through the heating zone of the first heating mechanism 2, so that the inner seamless metal tube and the outer seamless metal tube of the seamless metal composite tube billet are both heated to the first temperature. At this time, the temperature of the inner seamless metal tube and the outer seamless metal tube are the same. After that, the transfer mechanism 4 transfers the seamless metal composite tube billet heated by the first heating mechanism 2 from the first conveying mechanism 1 to the second conveying mechanism 3, and then the first driving mechanism 7 drives the seamless metal composite tube billet to pass through the heating zone of the ultrasonic induction heating mechanism 5 to heat the outer seamless metal tube of the seamless metal composite tube billet, so that the temperature of the outer seamless metal tube is further increased and then enters the three-roller cross rolling mechanism 6 for rolling. In this way, the outer seamless metal tube is heated to the second temperature, and the inner seamless metal tube of the seamless metal composite tube billet is heated to the third temperature by heat conduction of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, and the third temperature is greater than or equal to the first temperature. It should be noted that, since the ultrasonic induction heating mechanism 5 is sleeved on the outside of the seamless metal composite tube blank, according to the principle of ultrasonic induction heating, the ultrasonic induction heating mechanism 5 gradually heats the seamless metal composite tube blank from the outer layer to the inner layer, and the thickness of the ultrasonic induction heating can be controlled at a thinner thickness. Therefore, the outer seamless metal tube is subjected to ultrasonic induction heating to the second temperature, and then the ultrasonic induction heating is stopped. At this time, the induction heating of the inner seamless metal tube by the ultrasonic induction heating mechanism 5 is limited and can be ignored. The inner seamless metal tube is mainly heated by heat conduction of the heat of the outer seamless metal tube. At this time, the temperature of the inner seamless metal tube, that is, the third temperature, can remain unchanged or slightly increase, and the temperature increase is very small. This shows that the temperature of the inner seamless metal tube is lower than the temperature of the bonding interface between the outer seamless metal tube and the inner seamless metal tube, and the temperature of the bonding interface is lower than the temperature of the outer seamless metal tube, forming a seamless metal composite tube blank with a gradient temperature of the outer seamless metal tube-bonding interface-inner seamless metal tube. In this case, it is ensured that the outer seamless metal tube with high deformation resistance has a higher temperature during rolling, and the temperature of the inner seamless metal tube is not too high, which effectively inhibits the formation of brittle compounds at the bonding interface and improves the interface bonding strength of the seamless metal composite tube. At the same time, it avoids the inner seamless metal tube from being too high in temperature, which leads to the deterioration of the formability and oxidation resistance of the inner seamless metal tube, and improves the uneven wall thickness and poor surface quality of the seamless metal composite tube. In addition, during rolling, the outer seamless metal tube-bonding interface-inner seamless metal tube has a gradient temperature, which reduces the serious deformation incoordination phenomenon of the inner and outer seamless metal tubes, thereby effectively improving the interface bonding strength and reducing the head and tail cutting amount, thereby improving the yield rate.Furthermore, there is no need to lower the rolling temperature to avoid the need for higher rolling force during rolling, which would exceed the maximum rolling capacity that the three-roller oblique rolling mill can provide and cause rolling jams, thereby ensuring the forming quality of the seamless metal composite pipe, reducing the wear of the rolls and the rolling mill, and slowing down the rate of damage.
[0040] Taking the seamless steel / titanium composite tube as an example, it should be noted that in the embodiments provided by the present invention, when describing the seamless metal composite tubes of two materials, the seamless metal tube described first is located in the outer layer, and the seamless metal tube described later is located in the inner layer. Exemplarily, the seamless steel / titanium composite tube is a seamless metal composite tube in which the outer seamless metal tube is a seamless steel tube and the inner seamless metal tube is a seamless titanium tube. In specific implementation, the first heating mechanism 2 can be used to heat the temperature of the seamless steel tube and the seamless titanium tube of the seamless metal composite tube blank to a first temperature, and the first temperature is not higher than the phase change temperature of titanium. The ultrasonic induction heating mechanism 5 is used to heat the temperature of the outer seamless steel tube to the rolling temperature of steel (900℃-1200℃). On the one hand, it can prevent titanium from changing to β phase, and further avoid the generation of brittle compounds such as Fe-Ti at the bonding interface between the titanium tube and the steel tube, thereby improving the interface bonding strength, and ensuring the rolling temperature of the steel tube, thereby enhancing the bonding strength of the seamless steel / titanium composite tube. On the other hand, there is no need to use a lower rolling temperature to avoid the need for a higher rolling force during rolling, which would exceed the maximum rolling capacity that the three-roller oblique rolling mill can provide and cause rolling jams. Furthermore, the temperatures of seamless titanium tubes and seamless steel tubes are different, that is, the temperature of seamless steel tubes during rolling is greater than that of seamless titanium tubes, and there will be no serious deformation incoordination during the deformation process due to the large difference in performance between titanium and steel at the same temperature. Severe deformation incoordination will also cause the bonding interface to bear more shear force, which may rub apart the already bonded areas and cause interface failure. In addition, during the rolling process, the temperature of titanium is lower than 900°C, which will not cause uneven wall thickness and poor surface quality of the seamless steel / titanium composite tubes produced, so as not to affect subsequent use.
[0041] It should be noted that in the embodiments provided by the present invention, the seamless metal composite tube can also be a seamless metal composite tube with an outer layer of a seamless steel tube and an inner layer of a seamless aluminum tube, or an outer layer of a seamless titanium tube and an inner layer of a seamless copper tube, or an outer layer of a seamless titanium tube and an inner layer of a seamless aluminum tube. Of course, this is just an example and not a specific limitation. In addition, the first heating mechanism 2 provided in the embodiment of the present invention can be a heating furnace. Of course, the first heating mechanism 2 can also be a through-type induction heating mechanism. The seamless metal composite tube blank is uniformly heated to the same temperature as a whole by the heating furnace or the induction heating mechanism. The embodiment of the present invention adopts the combination of the first heating mechanism 2 and the ultrasonic induction heating mechanism 5 to quickly heat the outer seamless metal tube to a higher temperature, while the temperature of the inner seamless metal tube remains unchanged or slightly increases. The setting of the ultrasonic induction heating mechanism 5 makes the temperature of the outer seamless metal tube greater than the temperature of the inner seamless metal tube. Through short-term heat conduction, the temperature of the bonding interface between the outer seamless metal tube and the inner seamless metal tube is increased to form a seamless metal composite tube blank with a gradient temperature of the outer seamless metal tube-bonding interface-inner seamless metal tube. The deformation coordination performance of the seamless metal composite tube blank is improved by the gradient temperature difference, and the problem of insufficient rolling capacity of the rolling mill is overcome, which is conducive to the preparation of high-performance seamless metal composite tubes, reducing the amount of head and tail cut off when producing finished tubes, and reducing losses.
[0042] In a specific implementation, in one example, the second conveying mechanism 3 includes a second frame 31, a second drive motor 32, a third sprocket 33, a fourth sprocket 34, a third chain 35 and a plurality of V-shaped brackets 36 for carrying seamless metal composite tube blanks. The mounting end of the second drive motor 32 is fixedly mounted on the second frame 31, the third sprocket 33 is mounted on the output shaft of the second drive motor 32, the fourth sprocket 34 is rotatably mounted on the second frame 31, the third sprocket 33 and the fourth sprocket 34 are transmission-connected by the third chain 35, and a plurality of V-shaped brackets 36 are sequentially arranged on the third chain 35 along the conveying direction of the second conveying mechanism 3. When the output shaft of the second drive motor 32 rotates, the third sprocket 33 is synchronously driven to rotate. Under the action of the third chain 35, the fourth sprocket 34 rotates synchronously. When the output shaft of the second drive motor 32 rotates forward and reversely, multiple V-shaped brackets 36 are synchronously moved back and forth along the conveying direction of the second conveying mechanism 3 along with the third chain 35. When the V-shaped bracket 36 carries the seamless metal composite tube blank, it can drive the seamless metal composite tube blank to move in the direction close to the supersonic induction heating mechanism 5. It should be noted that when the seamless metal composite tube blank is placed on multiple V-shaped brackets 36, the axis of the seamless metal composite tube blank is parallel to the conveying direction of the second conveying mechanism 3.
[0043] It should be noted that see Figure 6As shown, the supersonic frequency induction heating mechanism 5 has a central circular hole for the seamless metal composite tube to pass through, and the central circular hole corresponds to the heating area of the supersonic frequency induction heating mechanism 5. A lifting frame is installed below the supersonic frequency induction heating mechanism 5, so that the height of the supersonic frequency induction heating mechanism 5 can be adjusted, so that the seamless metal composite tubes of different diameters are all located at the center of the central circular hole of the supersonic frequency induction heating mechanism 5 during the rolling process, ensuring that the outer seamless metal tube of the seamless metal composite tube is heated evenly.
[0044] In another example, see Figure 1 As shown, the first driving mechanism 7 includes a third frame 72, a chain driving structure 71 and a mandrel 73. The chain driving structure 71 is mounted on the third frame 72, and the mandrel 73 is mounted at the driving end of the chain driving structure 71. The length direction of the mandrel 73 extends along the conveying direction of the second conveying mechanism 3, and the chain driving structure 71 can drive the mandrel 73 to reciprocate along the conveying direction of the second conveying mechanism 3. When the second conveying mechanism 3 carries the seamless metal composite tube billet heated by the first heating mechanism 2, the chain driving structure 71 drives the mandrel 73 to move in the direction close to the seamless metal composite tube billet along the conveying direction of the second conveying mechanism 3, and makes the end of the mandrel 73 away from the chain driving structure 71 inserted into the seamless metal composite tube billet, and then the chain driving structure 71 continues to drive the mandrel 73 to drive the seamless metal composite tube billet to pass through the heating zone of the ultrasonic induction heating mechanism 5, and makes the seamless metal composite tube billet enter the three-roller cross rolling mechanism 6 for rolling. It is worth noting that the axis of the core rod 73, the axis of the seamless metal composite tube placed on the V-shaped bracket 36, the axis of the central circular hole of the ultrasonic induction heating mechanism 5 and the axis of the three-roller cross-rolling mechanism 6 can be colinear to ensure that the seamless metal composite tube can smoothly enter the three-roller cross-rolling mechanism 6.
[0045] In one possible implementation, reference Figures 3 to 5The first conveying mechanism 1 provided in the embodiment of the present invention comprises a first lifting frame 11, a plurality of first rotating rollers 12 arranged in parallel and along the conveying direction of the first conveying mechanism 1, a first sprocket 13, a first driving motor 14, a second sprocket 15, a first chain 16 and a second chain 17. The first lifting frame 11 has a first lifting end, a plurality of first rotating rollers 12 are arranged side by side, the axis of the first rotating roller 12 is perpendicular to the conveying direction of the first conveying mechanism 1, and the first rotating roller 12 is rotatably arranged at the first lifting end. Among them, the first heating mechanism 2 is arranged between two adjacent first rotating rollers 12. The first sprocket 13 corresponds to the first rotating roller 12, the first sprocket 13 is arranged at one end of the first rotating roller 12, the first driving motor 14 is arranged at the first lifting end, and the second sprocket 15 is arranged at the driving end of the first driving motor 14. The first sprocket 13 corresponding to one of the first rotating rollers 12 is connected to the second sprocket 15 through the first chain 16, and the first sprockets 13 corresponding to the plurality of first rotating rollers 12 are connected through the second chain 17.
[0046] Based on this, when the output shaft of the first driving motor 14 rotates, the second sprocket 15 is driven to rotate synchronously, and under the transmission action of the first chain 16, a first sprocket 13 corresponding to the first chain 16 is driven to rotate. Since the first sprockets 13 corresponding to the plurality of first rotating rollers 12 are connected by the second chain 17, when one first sprocket 13 rotates, under the action of the second chain 17, the plurality of first sprockets 13 can be driven to rotate, and accordingly, the plurality of first rotating rollers 12 are driven to rotate synchronously. When the seamless metal composite tube blank is carried on the first rotating roller 12, the rotation of the first rotating roller 12 can drive the seamless metal composite tube blank to move, so that the seamless metal composite tube blank passes through the heating zone of the first heating mechanism 2. The first heating mechanism 2 is arranged between two adjacent first rotating rollers 12. Similarly, the first heating mechanism 2 has a central circular hole for the seamless metal composite tube blank to pass through, and the central circular hole corresponds to the heating zone of the first heating mechanism 2. Under the action of the plurality of first rotating rollers 12, the seamless metal composite tube billet passes through the heating zone of the first heating mechanism 2, so that the first heating mechanism 2 heats the seamless metal composite tube billet. The number of the first heating mechanism 2 can be one, two, three or more. When the number of the first heating mechanism 2 is one, one first heating mechanism 2 is located between any two adjacent first rotating rollers 12. When the number of the first heating mechanism 2 is multiple, the multiple first heating mechanisms 2 are arranged at intervals. In other words, one or more first rotating rollers 12 are arranged between two adjacent first heating mechanisms 2.
[0047] The first lifting frame 11 can drive the multiple first rotating rollers 12 to rise and fall, so that the bearing surface of the first conveying mechanism 1 can match the heating area of the first heating mechanism 2, and ensure that the axis of the seamless metal composite tube billet is collinear with the axis of the central circular hole of the first heating mechanism 2 while ensuring that the seamless metal composite tube billet can pass through the heating area of the first heating mechanism 2, thereby improving the uniformity of heating of the seamless metal composite tube billet. When there are multiple first heating mechanisms 2, the first conveying mechanism 1 drives the seamless metal composite tube billet to pass through multiple first heating mechanisms 2 in sequence, which can ensure that the temperature of the seamless metal composite tube billet gradually rises to a preset temperature.
[0048] In a specific implementation, a recessed portion 121 is provided at a position of the first rotating roller 12 corresponding to the heating zone of the first heating mechanism 2, see Figure 5 , the recessed portion 121 is used to carry the seamless metal composite tube blank. Specifically, the recessed portion 121 can be a V-shaped groove opened in the circumferential direction of the first rotating roller 12. The setting of the recessed portion 121 ensures that the seamless metal composite tube blank is always in the middle position of the heating zone of the first heating mechanism 2 during the transmission process, so as to achieve uniform heating of the seamless metal composite tube blank. At the same time, it can ensure that seamless metal composite tube blanks of different diameters are always in the center of the heating zone during heating, avoiding uneven circumferential and axial bonding strength of the seamless metal composite tube blank caused by uneven temperature during rolling, which affects the use.
[0049] In an alternative approach, see Figure 2 and Figure 4 As shown, the transfer mechanism 4 includes a first frame 41, a bearing frame 42, two oppositely arranged turning frames 43 and an inclined plate 44. The bearing frame 42 is arranged on the first frame 41. The bearing frame 42 has a V-shaped groove for carrying the seamless metal composite tube blank. The length extension direction of the V-shaped groove is parallel to the conveying direction of the first conveying mechanism 1. The two oppositely arranged turning frames 43 are respectively rotated and arranged at the two ends of the length direction of the V-shaped groove. The turning frames 43 have a accommodating space matched with the V-shaped groove. The inclined plate 44 is connected to the bearing surface of the second conveying mechanism 3. One end of the inclined plate 44 is connected to the top of one side wall of the V-shaped groove, and the other end is inclined downward.
[0050] In specific implementation, after the first conveying mechanism 1 drives the seamless metal composite tube billet to pass through the heating zone of the first heating mechanism 2, the seamless metal composite tube billet is driven by the first conveying mechanism 1 to move to the V-shaped groove on the bearing frame 42. At this time, the two ends of the seamless metal composite tube billet are respectively located in the accommodating spaces of the two oppositely arranged flipping frames 43. The flipping frames 43 can be turned manually or driven to turn by a driving structure capable of driving the flipping frames 43 to rotate, so that the seamless metal composite tube billet slides off the inclined plate 44 and rolls onto the second conveying mechanism 3. In actual situations, one end of the inclined plate 44 is welded and fixed to the top of one side wall of the V-shaped groove, and the other end of the inclined plate 44 is close to the bearing surface of the second conveying mechanism 3, wherein the bottom of the end of the inclined plate 44 that is connected to the second conveying mechanism 3 is 1mm-5mm higher than the bearing surface of the second conveying mechanism 3, ensuring that the seamless metal composite tube billet can smoothly roll onto the second conveying mechanism 3.
[0051] In some embodiments, the gradient temperature-different three-roller cross-rolling equipment provided in the embodiment of the present invention further includes a cooling mechanism 8, which is arranged at the outlet end of the three-roller cross-rolling mechanism 6, and is used to cool the seamless metal composite pipe obtained after rolling. The cooling mechanism 8 may include a mounting frame 81, a liquid inlet 82 and a plurality of liquid outlets 83, and the mounting frame 81 is arranged at the outlet end of the three-roller cross-rolling mechanism 6. The mounting frame 81 has a through hole corresponding to the seamless metal composite pipe, and the liquid inlet 82 is arranged on the mounting frame 81 for providing cooling liquid. A plurality of liquid outlets 83 are arranged on the mounting frame 81 along the circumference of the through hole, and the plurality of liquid outlets 83 are connected with the liquid inlet 82, for receiving the cooling liquid, and outputting the cooling liquid to the seamless metal composite pipe after rolling. When the seamless metal composite pipe after rolling passes through the through hole, the cooling liquid is sprayed out from the liquid outlet 83 and sprayed on the seamless metal composite pipe, so as to cool the seamless metal composite pipe after rolling, and the cooling liquid may be water. Multiple liquid outlets 83 can be evenly arranged along the circumference of the through hole. When the rolled seamless metal composite pipe passes through the through hole, the axis of the seamless metal composite pipe coincides with the axis of the through hole, ensuring uniform cooling of the rolled seamless metal composite pipe.
[0052] In one example, the distance between the output end of the supersonic frequency induction heating mechanism 5 and the inlet end of the three-roller cross-rolling mechanism 6 is 10cm-50cm. In this way, the supersonic frequency induction heating mechanism 5 is arranged at 10cm-50cm from the entrance of the three-roller cross-rolling mill, and the gradient temperature heating of the outer seamless metal tube-bonding interface-inner seamless metal tube can be carried out synchronously with rolling, ensuring that the area of the seamless metal composite tube billet heated by the supersonic frequency induction heating mechanism 5 still has the ideal "outer seamless metal tube-bonding interface-inner seamless metal tube" gradient temperature effect during rolling. It avoids the situation that when the offline heating of the longer seamless metal composite tube billet is used, due to heat conduction, the outer seamless metal tube and the inner seamless metal tube exchange heat, and the seamless metal composite tube billet loses the gradient temperature effect before rolling or even reaches a uniform temperature. In actual situations, the number of turns and diameter of the coil of the supersonic frequency induction heating mechanism 5 can be changed to achieve gradient temperature heating of seamless metal composite tube billets with different diameters and different wall thickness combinations, and produce high-performance seamless metal composite tubes of different specifications. At the same time, the ultrasonic induction heating mechanism 5 is arranged on the rolling line, and the seamless metal composite tube billet after heating can immediately enter the three-roller cross-rolling mechanism 6. When the seamless metal composite tube billet is continuously rolled and fed, the gradient temperature of "outer seamless metal tube-bonding interface-inner seamless metal tube" is more stable, which can improve the uniformity of interface bonding strength and wall thickness. And the composite tube billet can be produced without length restrictions, and a seamless metal composite tube with a large aspect ratio can be produced. For example, the distance between the output end of the ultrasonic induction heating mechanism 5 and the inlet end of the three-roller cross-rolling mechanism 6 can be 10cm, 15cm, 20cm, 24cm, 30cm, 40cm, 50cm, etc., which is not specifically limited here.
[0053] The following describes the working principle of rolling a seamless steel / titanium composite pipe using the gradient temperature-differential three-roller cross-rolling equipment provided in an embodiment of the present invention in a possible implementation manner. Of course, this is not a specific limitation here.
[0054] First, the parameters of the first heating mechanism 2 are set according to the specific size of the seamless steel / titanium composite tube blank, and the conveying speed of the first conveying mechanism 1 is set to V0, and the seamless steel / titanium composite tube blank is placed on the first rotating roller 12 of the first conveying mechanism 1, so that the seamless steel / titanium composite tube blank passes through the heating zone of the first heating mechanism 2 at a speed of V0, so that the seamless steel / titanium composite tube blank is uniformly heated to the first temperature as a whole and then falls into the V-shaped groove of the transfer mechanism 4. Then, the seamless steel / titanium composite tube blank that is uniformly heated and has a temperature of the first temperature is turned over to the V-shaped bracket 36 of the second conveying mechanism 3 through the turning frame 43, and the chain driving structure 71 of the first driving mechanism 7 drives the mandrel 73 to move along the conveying direction of the second conveying mechanism 3. After the mandrel 73 is inserted into the seamless steel / titanium composite tube blank, the mandrel 73 continues to move forward until the head of the mandrel 73 passes through the cooling mechanism 8 and stops moving forward. Afterwards, the second driving motor 32 of the second conveying mechanism 3 drives the third chain 35 to rotate, driving the V-shaped bracket 36 fixed on the third chain 35 and the seamless steel / titanium composite tube blank placed on the V-shaped bracket 36 to move forward, so that the seamless steel / titanium composite tube blank passes through the heating zone of the ultrasonic induction heating mechanism 5 at a speed V1. Since the ultrasonic induction heating mechanism 5 is sleeved on the outside of the seamless steel / titanium composite tube blank, according to the principle of ultrasonic induction heating, the ultrasonic induction heating mechanism 5 gradually heats the seamless steel / titanium composite tube blank from the outer layer to the inner layer, and the ultrasonic induction heating The thickness can be controlled at a relatively thin thickness and can be heated quickly. Therefore, the outer layer of the steel tube is quickly heated to the second temperature by ultrasonic induction, and then the ultrasonic induction heating of the outer layer of the steel tube is stopped. At this time, the induction heating of the inner titanium tube by the ultrasonic induction heating mechanism is limited and can be ignored. The inner titanium tube is mainly heated by the heat conduction of the steel tube for a short time. The temperature of the inner titanium tube can remain unchanged or slightly increase. The temperature increase is very small. It is mainly because the bonding interface between the steel tube and the inner titanium tube will be heated by heat conduction, and the inner titanium tube has not reached the phase change temperature of the inner titanium tube. Adjust the motor speed of the three-roller oblique rolling mechanism 6, and ensure that the speed of the oblique rolling rollers of the three-roller oblique rolling mechanism 6 along the axial direction of the seamless steel / titanium composite tube is V2, and V2=V1. The seamless steel / titanium composite tube billet is kept at a forward speed of V1, and is pushed into the three-roller oblique rolling mechanism 6 for rolling and compounding. After the front end of the seamless steel / titanium composite tube billet contacts the oblique rolling roller, the entire seamless steel / titanium composite tube billet is driven by the oblique rolling roller to spirally advance at a speed of V1 and pass through the ultrasonic sensor and the rolling area in turn, so as to achieve gradient heating at different temperatures and rolling simultaneously. The seamless steel / titanium composite tube billet is driven by the oblique rolling roller to spirally advance at a speed of V1 and complete rolling, and then is cooled by the cooling mechanism 8 arranged at the outlet end of the three-roller oblique rolling mechanism 6, so that the temperature of the seamless steel / titanium composite tube is reduced to below 600°C, and a seamless steel / titanium composite tube with a large aspect ratio and good deformation coordination and excellent bonding performance is obtained.Finally, the finished pipe is prepared, the seamless steel / titanium composite pipe is subjected to low temperature annealing, sizing, and air cooling to room temperature, followed by straightening, cutting off the head and tail, and obtaining the finished seamless steel / titanium composite pipe, which is then bundled and packaged and waits for shipment. It should be noted that the speed V0 can range from 10mm / s-50mm / s, the temperature t1 can range from 650℃-850℃, the speed V1 can range from 30mm / s-100mm / s, and the temperature t2 can range from 900℃-1150℃. Titanium pipes include titanium and its alloy pipes, and steel pipes include carbon steel and alloy steel pipes.
[0055] In addition to the above, see Figure 8 The embodiment of the present invention further provides a method for preparing a seamless metal composite pipe. Based on the above-mentioned gradient temperature-different three-roller cross-rolling equipment, the method for preparing a seamless metal composite pipe provided by the embodiment of the present invention comprises the following steps:
[0056] Step S1, providing a seamless metal composite tube blank, wherein the seamless metal composite tube blank comprises an inner seamless metal tube and an outer seamless metal tube which are coaxially sleeved;
[0057] Step S2, heating the seamless metal composite tube blank so that both the inner seamless metal tube and the outer seamless metal tube are heated to a first temperature;
[0058] Step S3, performing ultrasonic induction heating on the outer seamless metal tube of the seamless metal composite tube blank, so that the outer seamless metal tube is heated to a second temperature, and the inner seamless metal tube is heated to a third temperature by heat conduction of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, the third temperature is greater than or equal to the first temperature, and the bonding interface temperature between the outer seamless metal tube and the inner seamless metal tube is between the third temperature and the second temperature;
[0059] Step S4, rolling the seamless metal composite tube blank to obtain a seamless metal composite tube.
[0060] When the above technical solution is adopted, the seamless metal composite tube blank is heated so that the inner seamless metal tube and the outer seamless metal tube of the seamless metal composite tube blank are both heated to the first temperature, and then the outer seamless metal tube of the seamless metal composite tube blank is subjected to ultrasonic induction heating, the outer seamless metal tube is heated to the second temperature, and the inner seamless metal tube of the seamless metal composite tube blank is heated to the third temperature by heat conduction heating of the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, the third temperature is greater than or equal to the first temperature, and the temperature of the bonding interface between the outer seamless metal tube and the inner seamless metal tube is between the third temperature and the second temperature. This indicates that the temperature of the inner seamless metal tube is lower than the temperature of the bonding interface between the outer seamless metal tube and the inner seamless metal tube, and at the same time, the temperature of the bonding interface is lower than the temperature of the outer seamless metal tube, forming a seamless metal composite tube blank with a gradient temperature of the outer seamless metal tube-bonding interface-inner seamless metal tube. In this case, it is ensured that the outer seamless metal tube has a higher temperature during rolling, and the temperature of the inner seamless metal tube is not too high, which effectively inhibits the formation of brittle compounds at the bonding interface and improves the interface bonding strength of the seamless metal composite tube. At the same time, it avoids the inner seamless metal tube from having a too high temperature, which leads to the deterioration of the formability and oxidation resistance of the inner seamless metal tube, and improves the uneven wall thickness and poor surface quality of the seamless metal composite tube. In addition, during rolling, the outer seamless metal tube-bonding interface-inner seamless metal tube has a gradient temperature, which reduces the serious deformation incoordination of the inner and outer seamless metal tubes, thereby effectively improving the interface bonding strength and reducing the head and tail resection amount, thereby improving the yield rate. Furthermore, there is no need to reduce the rolling temperature to ensure the forming quality of the seamless metal composite tube, reduce the wear of the rollers and rolling mills, and slow down the damage rate.
[0061] In specific implementation, when the outer seamless metal tube of the seamless metal composite tube blank is heated, the heating depth can be 1 / 4-3 / 4 of the wall thickness of the outer seamless metal tube, which is adjusted according to the specific wall thickness of the seamless metal composite tube blank. In addition, in step S4: rolling the seamless metal composite tube blank to obtain the seamless metal composite tube, the method for preparing the seamless metal composite tube provided in the embodiment of the present application also includes step S5: processing the seamless metal composite tube, such as sizing, cooling, straightening, cutting off the head and tail of the seamless metal composite tube to obtain a finished seamless metal composite tube.
[0062] It should be noted that the preparation method of the seamless metal composite pipe provided in the embodiment of the present invention can be based on the gradient temperature-differential three-roller cross-rolling equipment provided in the embodiment of the present invention. Of course, other equipment that can realize the preparation method of the seamless metal composite pipe provided in the embodiment of the present invention can also be used, and no specific limitation is made here.
[0063] In a possible implementation, in step S1, a seamless metal composite tube blank is provided, wherein the seamless metal composite tube includes an inner seamless metal tube and an outer seamless metal tube that are coaxially sleeved, and the steps are as follows:
[0064] Step S11, providing an inner seamless metal tube and an outer seamless metal tube of different materials;
[0065] Step S12, pre-treating the inner seamless metal tube and the outer seamless metal tube;
[0066] Step S13, sleeve the outer seamless metal tube over the inner seamless metal tube;
[0067] Step S14, welding the two ends of the outer seamless metal tube and the inner seamless metal tube to obtain a seamless metal composite tube blank.
[0068] In the specific implementation, firstly, an inner seamless metal tube and an outer seamless metal tube of different materials are provided, and the inner and outer walls of the two seamless metal tubes are polished to remove the oxide layer and oil stains on the two seamless metal tubes, and then a high-pressure air gun is used to blow away the debris remaining on the surface to be combined. The outer seamless metal tube is sleeved outside the inner seamless metal tube. At this time, the inner seamless metal tube and the outer seamless metal tube can be interference fit. Of course, in the radial direction, there can be a gap between the inner wall of the outer seamless metal tube and the outer wall of the inner seamless metal tube, and the gap can be 0-1mm. The joint interface of the two ends of the sleeved inner seamless metal tube and the outer seamless metal tube is welded and sealed, and further a stainless steel exhaust pipe can be welded at one end, so that the joint interface of the two seamless metal tubes can be vacuumed through the exhaust pipe. In addition, it should be noted that before vacuuming, a layer of high temperature resistant sealant can be evenly applied on the weld to prevent air leakage. After vacuuming, the exhaust pipe is sealed, so that a seamless metal composite tube blank is obtained.
[0069] In some embodiments, the first temperature is 300°C-850°C, the second temperature is 600°C-1200°C, and the third temperature is 300-900°C. In this way, the outer seamless metal tube-bonding interface-inner seamless metal tube of the seamless metal composite tube blank forms a gradient temperature difference before rolling. In specific implementation, the first temperature can be 300°C, 360°C, 400°C, 450°C, 500°C, 600°C, 750°C, 850°C, etc. The second temperature can be 600°C, 700°C, 800°C, 90°C, 1000°C, 1200°C, etc. The third temperature can be 300°C, 340°C, 400°C, 450°C, 500°C, 600°C, 750°C, 900°C. Of course, this is just an example and is not a specific limitation. It is determined according to the actual material of the inner and outer seamless metals.
[0070] Taking seamless steel / titanium composite tube as an example, the outer seamless metal tube is a seamless steel tube, and the inner seamless metal tube is a seamless titanium tube. The temperature of the seamless titanium tube can be heated to 650℃-850℃, and the temperature of the seamless steel tube can be heated to 900℃-1150℃. In this way, when the temperature of the seamless titanium tube is 650℃-850℃, it is lower than the phase transition temperature of titanium (882℃), avoiding the transformation of the close-packed hexagonal α phase to the body-centered cubic β phase, and further avoiding the formation of brittle compounds such as Fe-Ti at the interface between the seamless titanium tube and the seamless steel tube, which greatly reduces the interface bonding strength. At the same time, the temperature of the seamless steel tube is 900℃-1150℃, which meets the rolling deformation temperature of steel. In this way, while ensuring the bonding strength, the deformation of the seamless steel tube and the seamless titanium tube is more coordinated, the deformation resistance of the two materials is closer, and synchronous and coordinated deformation is achieved.
[0071] The preparation method of the seamless metal composite pipe provided in the present application is described below with three specific embodiments, which are of course not specifically limited here.
[0072] Example 1
[0073] Step S1, providing a seamless metal composite tube blank: preparing a seamless 304 stainless steel tube with a length of 1m, an outer diameter of 70mm, and a wall thickness of 5mm and a seamless TA2 tube with a length of 1m, an outer diameter of 60.1mm, and a wall thickness of 3mm, and processing grooves at both ends of the seamless 304 stainless steel tube. The inner surface of the seamless 304 stainless steel tube and the outer surface of the seamless TA2 tube are respectively polished by a fully automatic tube polishing machine to remove the surface oxide layer and oil stains, etc. After polishing, a high-pressure air gun is used to blow away the debris remaining on the surface to be combined. The polished seamless tube blank is assembled in the manner of seamless 304 stainless steel tube outside and seamless TA2 tube inside, and then the two ends of the tube blank after the assembly are sealed and welded with 1.6mm copper-nickel welding wire (ERCUNI welding wire) and a stainless steel exhaust pipe with a length of 15mm and a diameter of 6mm is welded at one end, so that the interface of the two seamless metal tubes can be vacuumed through the exhaust pipe. In addition, it should be noted that before vacuuming, a layer of high temperature resistant sealant is evenly applied on the weld to prevent air leakage. After vacuuming, the vacuum pipe is sealed to make a seamless 304 / TA2 composite tube blank.
[0074] Step S2, heating the seamless metal composite tube blank: At this time, an air heating furnace can be used to heat the seamless 304 / TA2 composite tube blank. The heating temperature of the air heating furnace can be set to 700°C. After the furnace temperature reaches 700°C and stabilizes, the seamless 304 / TA2 composite tube blank is placed in the air heating furnace for heating and kept warm for 1 hour.
[0075] Step S3, heating the outer metal tube of the seamless metal composite tube blank: placing an induction heating coil with an inner hole diameter of 90 mm at the entrance of the three-roller oblique rolling mechanism 6, and ensuring that the axis of the induction heating coil coincides with the axis of the mandrel 73 during placement. The power of the coil of the ultrasonic induction heating mechanism 5 is 300KW and the frequency is 30KHZ. After setting the induction heating temperature to 1100°C, start the power supply, transfer the seamless 304 / TA2 composite tube blank heated by the air heating furnace to the V-shaped bracket 36 of the second conveying mechanism 3, and then drive the mandrel 73 forward through the chain drive structure 71 to insert the mandrel 73 with a diameter of 50 mm into the seamless 304 / TA2 composite tube blank. After that, the mandrel 73 continues to move forward until the head of the mandrel 73 passes through the cooling mechanism 8 and stops moving forward. Afterwards, the second driving motor 32 of the second conveying mechanism 3 drives the third chain 35 to rotate, driving the V-shaped bracket 36 fixed on the third chain 35 and the seamless 304 / TA2 composite tube blank placed on the V-shaped bracket 36 to pass through the ultrasonic induction heating wire mechanism at a speed of 40 mm / s, and heats the outer layer of the outer seamless 304 stainless steel tube to about 1100°C within a depth of 2 mm, which is higher than the temperature of the inner seamless TA2 tube, and the temperature of the inner seamless TA2 tube does not exceed the phase change temperature.
[0076] Step S4, rolling the seamless metal composite tube billet to obtain a seamless metal composite tube: by adjusting the positions of the oblique rolling rollers and the guide plates in the three-roll oblique rolling mechanism 6, the diameter of the target hole type (i.e., the entrance end of the three-roll oblique rolling mechanism 6) is made to be 62 mm, and the motor speed is set to 240 rpm, so that the oblique rolling roller speed component along the axial direction of the seamless 304 / TA2 composite tube billet is 40 mm / s. The second conveying mechanism 3 drives the seamless 304 / TA2 composite tube billet into the three-roll oblique rolling mechanism 6 at a speed of 40 mm / s, and continues to spirally advance at a speed of 40 mm / s driven by the oblique rolling rollers and completes the rolling to obtain a seamless 304 / TA2 composite tube with a large aspect ratio. Compared with the seamless 304 / TA2 composite tube prepared by the ordinary hot rolling method in which the seamless 304 / TA2 composite tube billet is uniformly heated to 950°C in the prior art, the deformation coordination is greatly improved. Comparison Fig. 9 and Fig.10 As shown, by observing the bonding interface in the middle of the seamless 304 / TA2 composite pipe, Fig. 9 As shown in the figure, the seamless 304 / TA2 composite tube prepared by the ordinary hot rolling method provided by the prior art has obvious element diffusion at the bonding interface, and the compound layer at the bonding interface produces defects such as cracks and interface cracking during the spiral rolling process, and the interface bonding strength is 95MPa. Fig.10 The seamless 304 / TA2 composite tube prepared by the preparation method of the seamless metal composite tube provided by the present application has good bonding interface, no obvious cracks, pores and other defects, no obvious element diffusion layer is observed on the interface, and the interface bonding strength reaches 190MPa.
[0077] Step S5, processing the seamless metal composite pipe: sizing the prepared seamless 304 / TA2 composite pipe and air cooling it to a certain temperature, then straightening it and cutting off the head and tail to obtain the finished seamless 304 / TA2 composite pipe, which is then bundled and packaged and waited for shipment.
[0078] Example 2
[0079] Step S1, providing a seamless metal composite tube blank: preparing a seamless 45 steel tube with a length of 0.5m, an outer diameter of 70mm, and a wall thickness of 6.5mm and a seamless TA2 tube with a length of 0.5m, an outer diameter of 57mm, and a wall thickness of 3mm, and processing grooves at both ends of the seamless 45 steel tube. The inner surface of the seamless 45 steel tube and the outer surface of the seamless TA2 tube are respectively polished by a fully automatic pipe polishing machine to remove the surface oxide layer and oil stains, etc. After polishing, a high-pressure air gun is used to blow away the debris remaining on the surface to be combined. The polished tube blank is assembled in the manner of seamless 45 steel tube outside and seamless TA2 tube inside, and then the two ends of the tube blank after the assembly are sealed and welded with 1.6mm copper-nickel welding wire (ERCUNI welding wire) and a stainless steel exhaust pipe with a length of 15mm and a diameter of 8mm is welded at one end, so that the interface of the two seamless metal tubes can be vacuumed through the exhaust pipe. In addition, it should be noted that before vacuuming, a layer of high temperature resistant sealant is evenly applied on the weld to prevent air leakage. After vacuuming, the vacuum pipe is sealed to make a seamless 45 steel / TA2 composite tube blank.
[0080] Step S2, heating the seamless metal composite tube billet: setting the heating temperature of the air heating furnace to 750°C, waiting for the furnace temperature to reach 750°C and stabilize, placing the seamless 45 steel / TA2 composite tube billet in the air heating furnace for heating, and keeping it warm for 1.5 hours.
[0081] Step S3, heating the outer seamless metal tube of the seamless metal composite tube blank: placing an induction heating coil with an inner hole diameter of 90 mm at the entrance of the three-roller oblique rolling mechanism 6, and ensuring that the axis of the induction heating coil coincides with the axis of the mandrel 73 during placement. The power of the coil of the ultrasonic induction heating mechanism 5 is 260KW and the frequency is 20KHZ. After setting the induction heating temperature to 950°C, start the power supply, transfer the seamless 45 steel / TA2 composite tube blank heated by the air heating furnace to the V-shaped bracket 36 of the second conveying mechanism 3, and then drive the mandrel 73 forward through the chain drive structure 71. After the mandrel 73 with a diameter of 46 mm is inserted into the seamless 45 steel / TA2 composite tube blank, the mandrel 73 continues to move forward until the head of the mandrel 73 passes through the cooling mechanism 8 and stops moving forward. Afterwards, the second driving motor 32 of the second conveying mechanism 3 drives the third chain 35 to rotate, driving the V-shaped bracket 36 fixed on the third chain 35 and the seamless 45 steel / TA2 composite tube blank placed on the V-shaped bracket 36 to pass through the ultrasonic induction heating wire mechanism at a speed of 50mm / s, and heats the outer surface of the outer seamless 45 steel tube to 950°C within a depth of 4mm, which is higher than the temperature of the inner seamless TA2 tube, and the temperature of the inner seamless TA2 tube does not exceed the phase change temperature.
[0082] Step S4, rolling seamless metal composite tube billets to obtain seamless metal composite tubes: by adjusting the positions of the oblique rolling rollers and guide plates in the three-roll oblique rolling mechanism 6, the target hole type (i.e., the entrance end of the three-roll oblique rolling mechanism 6) is 58 mm in diameter, the motor speed is set to 300 rpm, and the oblique rolling roller speed is 50 mm / s along the axial direction of the seamless 45 steel / TA2 composite tube billet. The second conveying mechanism 3 drives the seamless 45 steel / TA2 composite tube billet into the three-roll oblique rolling mechanism 6 at a speed of 50 mm / s, and continues to spiral forward at a speed of 50 mm / s under the drive of the oblique rolling rollers and completes the rolling to obtain a large aspect ratio seamless 45 steel / TA2 composite tube. Compared with the seamless 45 steel / TA2 composite tube prepared by the ordinary hot rolling method in which the seamless 45 steel / TA2 composite tube billet is uniformly heated to 950°C in the prior art, the deformation coordination is greatly improved. By observing the bonding interface in the middle of the seamless 45 steel / TA2 composite pipe, it is found that the bonding interface of the seamless 45 steel / TA2 composite pipe prepared by the ordinary hot rolling method provided by the prior art has obvious element diffusion, and the compound layer at the bonding interface has defects such as cracks and interface cracking during the spiral rolling process, and the interface bonding strength is 110MPa. The seamless 45 steel / TA2 composite pipe prepared by the preparation method of the seamless metal composite pipe provided by the present application has good bonding interface, no obvious cracks, pores and other defects, no obvious element diffusion layer is observed at the interface, and the interface bonding strength reaches 200MPa.
[0083] Step S5, processing the seamless metal composite pipe: sizing the prepared seamless 45 steel / TA2 composite pipe and air cooling it to a certain temperature, then straightening it and cutting off the head and tail to obtain a finished seamless 45 steel / TA2 composite pipe, which is then bundled and packaged and waited for shipment.
[0084] Example 3
[0085] Step S1, providing a seamless metal composite tube blank: preparing a seamless 304 stainless steel tube with a length of 1m, an outer diameter of 76mm, and a wall thickness of 6mm and a seamless T2 copper tube with a length of 1m, an outer diameter of 64.1mm, and a wall thickness of 3mm, and processing grooves at both ends of the seamless 304 stainless steel tube. The inner surface of the seamless 304 stainless steel tube and the outer surface of the seamless T2 copper tube are polished by a fully automatic tube polishing machine to remove the surface oxide layer and oil stains, etc. After polishing, a high-pressure air gun is used to blow away the debris remaining on the surface to be combined. The polished tube blank is assembled in the manner of seamless 304 stainless steel tube outside and seamless T2 copper tube inside, and then the two ends of the tube blank after the assembly are sealed and welded with 1.6mm chromium-nickel stainless steel welding wire and a stainless steel exhaust pipe with a length of 15mm and a diameter of 8mm is welded at one end, so that the interface of the two seamless metal tubes can be vacuumed through the exhaust pipe. In addition, it should be noted that before vacuuming, a layer of high temperature resistant sealant is evenly applied on the weld to prevent air leakage. After vacuuming, the vacuum pipe is sealed to make a seamless 304 / T2 copper composite tube blank.
[0086] Step S2, heating the seamless metal composite tube billet: setting the heating temperature of the air heating furnace to 500°C, waiting for the furnace temperature to reach 500°C and stabilize, placing the seamless 304 / T2 copper composite tube billet in the air heating furnace for heating, and keeping it warm for 1.5 hours.
[0087] Step S3, heating the outer seamless metal tube of the seamless metal composite tube blank: placing an induction heating coil with an inner hole diameter of 95mm at the entrance of the three-roller oblique rolling mechanism 6, and ensuring that the axis of the induction heating coil coincides with the axis of the mandrel 73 during placement. The power of the coil of the ultrasonic induction heating mechanism 5 is 250KW and the frequency is 25KHZ. After setting the induction heating temperature to 1000℃, start the power supply, transfer the seamless 304 / T2 copper composite tube blank heated by the air heating furnace to the V-shaped bracket 36 of the second conveying mechanism 3, and then drive the mandrel 73 forward through the chain drive structure 71 to insert the mandrel 73 with a diameter of 54mm into the seamless 304 / T2 copper composite tube blank. After that, the mandrel 73 continues to move forward until the head of the mandrel 73 passes through the cooling mechanism 8 and stops moving forward. Afterwards, the second driving motor 32 of the second conveying mechanism 3 drives the third chain 35 to rotate, driving the V-shaped bracket 36 fixed on the third chain 35 and the seamless 304 / T2 copper composite tube blank placed on the V-shaped bracket 36 to pass through the ultrasonic induction heating wire mechanism at a speed of 40mm / s, and heats the outer layer of the outer seamless 304 stainless steel tube to 1000℃ within a depth of 5mm, which is higher than the temperature of the inner seamless T2 copper tube. The temperature of the inner seamless T2 copper tube remains basically unchanged at 500℃.
[0088] Step S4, rolling seamless metal composite tube billet to obtain seamless metal composite tube: by adjusting the position of the oblique rolling roller and the guide plate in the three-roller oblique rolling mechanism 6, the diameter of the target hole type (i.e., the entrance end of the three-roller oblique rolling mechanism 6) is 66mm, the motor speed is set to 240 revolutions, and the oblique rolling roller speed along the axial direction of the seamless 304 / T2 copper composite tube billet is 40mm / s. The second conveying mechanism 3 drives the seamless 304 / T2 copper composite tube billet into the three-roller oblique rolling mechanism 6 at a speed of 40mm / s, and continues to spiral forward at a speed of 40mm / s under the drive of the oblique rolling roller and completes the rolling, to obtain a seamless 304 / T2 copper composite tube with a large aspect ratio. Compared with the seamless 304 / T2 copper composite tube prepared by the ordinary hot rolling method in which the seamless 304 / T2 copper composite tube billet is uniformly heated to 1000°C in the prior art, the deformation coordination is greatly improved. By observing the bonding interface in the middle of the seamless 304 / T2 copper composite tube, the bonding strength of the seamless 304 / T2 copper composite tube prepared by the common hot rolling method provided by the prior art is 32MPa. The seamless 304 / T2 copper composite tube prepared by the preparation method of the seamless metal composite tube provided by the present application has a good bonding interface, without obvious defects such as cracks and pores, and the interface bonding strength reaches 48MPa.
[0089] Step S5, processing the seamless metal composite pipe: sizing the prepared seamless 304 / T2 copper composite pipe and air cooling it to a certain temperature, then straightening it and cutting off the head and tail to obtain a finished seamless 304 / T2 copper composite pipe, which is then bundled and packaged and waited for shipment.
[0090] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.
[0091] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A gradient temperature-different three-roller cross-rolling equipment, characterized in that: include: A first conveying mechanism, used for carrying a seamless metal composite tube blank; a first heating mechanism, wherein the first conveying mechanism is further used to drive the seamless metal composite tube blank through a heating zone of the first heating mechanism, and the first heating mechanism is used to heat both the inner seamless metal tube and the outer seamless metal tube of the seamless metal composite tube blank to a first temperature; A second conveying mechanism, used for carrying the seamless metal composite tube blank heated by the first heating mechanism; a transfer mechanism, used for receiving the seamless metal composite tube blank heated by the first heating mechanism, and transferring the seamless metal composite tube blank to the bearing surface of the second conveying mechanism; an ultrasonic induction heating mechanism, used for heating the outer seamless metal tube of the seamless metal composite tube blank heated by the first heating mechanism to a second temperature, and the inner seamless metal tube of the seamless metal composite tube blank is heated by heat conduction of the outer seamless metal tube to a third temperature, wherein the second temperature is greater than the first temperature and the third temperature, and the third temperature is greater than or equal to the first temperature; A three-roller cross-rolling mechanism is used to roll the seamless metal composite tube billet heated by the ultrasonic induction heating mechanism; The first driving mechanism is used to drive the seamless metal composite tube blank on the second conveying mechanism to pass through the heating zone of the ultrasonic induction heating mechanism and enter the three-roller cross-rolling mechanism.
2. The gradient temperature-different three-roller cross-rolling equipment according to claim 1 is characterized in that: The first conveying mechanism comprises: A first lifting frame having a first lifting end; A plurality of first rotating rollers are arranged in parallel with each other and along the conveying direction of the first conveying mechanism, wherein the axes of the first rotating rollers are perpendicular to the conveying direction; the first rotating rollers are rotatably arranged at the first lifting end; wherein the first heating mechanism is arranged between two adjacent first rotating rollers; a first sprocket, corresponding to the first rotating roller and disposed at one end of the first rotating roller; A first driving motor, disposed at the first lifting end; A second sprocket, disposed at a driving end of the first driving motor; A first chain, wherein the first sprocket corresponding to one of the first rotating rollers is connected to the second sprocket through the first chain transmission; A second chain, the first sprockets corresponding to the plurality of first rotating rollers are connected to each other through the second chain transmission.
3. The gradient temperature-different three-roller cross-rolling equipment according to claim 2 is characterized in that: A recessed portion is provided at a position of the first rotating roller corresponding to the heating zone of the first heating mechanism, and the recessed portion is used to carry the seamless metal composite tube blank.
4. The gradient temperature-different three-roller cross-rolling equipment according to claim 1 is characterized in that: The transfer mechanism includes: First rack; A carrier frame, arranged on the first frame, the carrier frame having a V-shaped groove for carrying the seamless metal composite tube blank; Two flip frames are arranged opposite to each other and are rotatably arranged at two ends of the length direction of the V-shaped groove respectively; the flip frames have a receiving space matched with the V-shaped groove; The inclined plate is connected to the bearing surface of the second conveying mechanism; one end of the inclined plate is connected to the top of one side wall of the V-shaped groove, and the other end is inclined downward.
5. The gradient temperature-different three-roller cross-rolling equipment according to claim 1 is characterized in that: The gradient temperature-different three-roller cross-rolling equipment also includes a cooling mechanism, which is arranged at the outlet end of the three-roller cross-rolling mechanism and is used to cool the seamless metal composite pipe obtained after rolling.
6. The gradient temperature-different three-roller cross-rolling equipment according to claim 5, characterized in that: The cooling mechanism comprises: A mounting frame is arranged at the outlet end of the three-roller cross-rolling mechanism; the mounting frame has a through hole corresponding to the seamless metal composite pipe; A liquid inlet, disposed on the mounting frame, for providing cooling liquid; A plurality of liquid outlets are arranged on the mounting frame along the circumference of the through hole; the plurality of liquid outlets are connected with the liquid inlet, and are used to receive the coolant and output the coolant to the seamless metal composite pipe.
7. The gradient temperature-different three-roller cross-rolling equipment according to claim 1 is characterized in that: The distance between the output end of the ultrasonic induction heating mechanism and the inlet end of the three-roller cross-rolling mechanism is 10 cm-50 cm.
8. A method for preparing a seamless metal composite pipe, based on the gradient temperature-differential three-roller cross-rolling equipment according to any one of claims 1 to 7, characterized in that: The method for preparing the seamless metal composite pipe comprises: A seamless metal composite tube blank is provided, wherein the seamless metal composite tube blank comprises an inner seamless metal tube and an outer seamless metal tube which are coaxially sleeved; Heating the seamless metal composite tube blank so that both the inner seamless metal tube and the outer seamless metal tube are heated to a first temperature; Performing ultrasonic induction heating on the outer seamless metal tube of the seamless metal composite tube blank, so that the outer seamless metal tube is heated to a second temperature, and the inner seamless metal tube is heated to a third temperature by heat conduction from the outer seamless metal tube, wherein the second temperature is greater than the first temperature and the third temperature, the third temperature is greater than or equal to the first temperature, and the bonding interface temperature between the outer seamless metal tube and the inner seamless metal tube is between the third temperature and the second temperature; The seamless metal composite tube blank is rolled to obtain a seamless metal composite tube.
9. The method for preparing a seamless metal composite pipe according to claim 8, characterized in that: The present invention provides a seamless metal composite tube blank, wherein the seamless metal composite tube comprises an inner seamless metal tube and an outer seamless metal tube which are coaxially sleeved and include: Providing the inner seamless metal tube and the outer seamless metal tube of different materials; Pre-treating the inner seamless metal tube and the outer seamless metal tube; The outer seamless metal tube is sleeved outside the inner seamless metal tube; The two ends of the outer seamless metal tube and the inner seamless metal tube are welded to obtain the seamless metal composite tube blank.
10. The method for preparing a seamless metal composite pipe according to claim 8, characterized in that: The first temperature is 300°C-850°C; The second temperature is 600°C-1200°C; The third temperature is 300-900°C.
Citation Information
Patent Citations
Cooling spray nozzle and through-water cooling device
CN103252366A
Large-length-diameter-ratio dissimilar metal composite thin-walled tube progressive skew rolling composite equipment and method thereof
CN115608784A
Seamless metal composite pipe interface thermal controllable continuous rolling equipment and method
CN116393515A
Pipe fitting conveying mechanism of steel pipe production line
CN209427532U
Cache discharging and conveying device for steel pipes
CN215515652U