Chromium-zirconium-tungsten compound carbide strengthened and toughened WC-Co hard alloy and preparation method thereof

By using Cr2O3, ZrO2, WO3 to form complex carbides in WC-Co cemented carbides, and sintering them with WC and Co at high temperature and high pressure to refine the grains, the WC-Co cemented carbides were solved during the sintering process. The problem of abnormal growth of WC grains achieves the effect of high hardness and high toughness of the material.

CN118926520APending Publication Date: 2024-11-12CHINA NONFERROUS METALS (GUILIN) GEOLOGY AND MINING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985311.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

WC-Co carbides grow abnormally during sintering, resulting in the inherent contradiction of high hardness, strength and toughness of the material, making it difficult to have both high hardness and high strength and toughness.

Method used

By ball milling and mixing Cr2O3, ZrO2, WO3 with carbon black, vacuum hot carbon reduction is carried out to form a complex carbide, and high-temperature and high-pressure sintering with WC and Co, it promotes the dispersion and solid-state reaction between ZrC, Cr3C2 and WC. To improve the dislocation density and mechanical properties.

Benefits of technology

It has achieved both high hardness and high toughness of WC-Co carbide, with Vickers hardness reaching 1885~1925HV and fracture toughness of 13.8~14.2MPa·m1/2, meeting the practical application needs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a chromium-zirconium-tungsten compound carbide strengthened and toughened WC-Co hard alloy and a preparation method thereof, and belongs to the field of hard alloy materials. According to the preparation method provided by the invention, Cr2O3, ZrO2, WO3 and carbon black are subjected to a reduction reaction to form a compound carbide, and grains can be refined to improve the dislocation density, so that the hardness of the material is improved; the compound carbide and a mixture of WC powder and Co are subjected to high-temperature and high-pressure sintering, dispersion among different carbides is promoted, the grain growth time is shortened, and the grain size is further refined; and continuous growth of crystal grains can be limited through high-temperature and high-pressure sintering, and growth of the crystal grains is inhibited, so that the obtained WC-Co hard alloy has high hardness, high strength and high toughness. The result of the embodiment shows that the Vickers hardness of the WC-Co hard alloy obtained by the preparation method provided by the invention is 1885-1925 HV, and the fracture toughness of the WC-Co hard alloy obtained by the preparation method provided by the invention is 13.8-14.2 MPa.m < 1 / 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cemented carbide materials, and in particular to a chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide and a preparation method thereof. Background Art

[0002] Cemented carbide is a material with high strength and high wear resistance produced by powder metallurgy process of hard phase and binder phase. WC-Co cemented carbide is widely used in aerospace, electronics, engineering machinery and mining due to its comprehensive properties of high hardness, high strength and high wear resistance, and is known as the "teeth of industry". However, hard materials are brittle materials. As we all know, WC-Co cemented carbide has an inherent contradiction of high hardness but low strength and toughness, or high strength and toughness but low hardness due to the abnormal growth of WC grains during sintering.

[0003] The use of carbides to modify WC-Co cemented carbide can improve the toughness of WC-Co cemented carbide; for example, CN114574727A discloses the use of chromium-vanadium-tungsten composite carbides to modify WC-based cemented carbide, and the Vickers hardness of the obtained WC-based cemented carbide can reach 1670MPa, the bending strength can reach 2835MPa, and the fracture toughness can reach 15.1MPa·m 1 / 2 , but it still cannot meet the needs of practical applications. Summary of the invention

[0004] The purpose of the present invention is to provide a chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide and a preparation method thereof. The preparation method provided by the present invention enables the WC-Co cemented carbide to have both high hardness and high toughness.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide, comprising the following steps:

[0007] (1) Cr 2 O 3 、ZrO 2 , WO 3 After ball milling with carbon black, vacuum hot carbon reduction is performed to obtain a complex carbide;

[0008] (2) ball-milling the complex carbide obtained in step (1) with WC and Co to obtain a mixture;

[0009] (3) The mixture obtained in step (2) is subjected to high temperature and high pressure sintering to obtain chromium-zirconium-tungsten composite carbide-reinforced WC-Co cemented carbide.

[0010] Preferably, the Cr in step (1) 2 O 3 、ZrO 2 , WO 3 The molar ratio of carbon black is 1:(0.3~3):(0.1~3):(0.3~1).

[0011] Preferably, the rotation speed of the ball milling mixing in the step (1) is 800-1200 r / min, the ball milling mixing time is 2-5 h, and the ball-to-material ratio of the ball milling mixing is (1-6):1.

[0012] Preferably, the temperature of the vacuum hot carbon reduction in step (1) is 1400-1600°C, the time of the vacuum hot carbon reduction is 1-5 hours, and the vacuum degree of the vacuum hot carbon reduction is 10 -1 ~10 -3 Pa.

[0013] Preferably, the mass ratio of the complex carbide to WC and Co in step (2) is (0.1-1): (84-94.9): (5-15).

[0014] Preferably, the rotation speed of the ball milling mixing in the step (2) is 200-500 r / min, the ball milling mixing time is 2-12 h, and the ball-to-material ratio of the ball milling mixing is (3-8):1.

[0015] Preferably, the mixture obtained in step (2) is subjected to high-temperature vacuum treatment before the high-temperature and high-pressure sintering in step (3).

[0016] Preferably, the temperature of the high temperature vacuum treatment is 800-1200°C, the time of the high temperature vacuum treatment is 1-3 hours, and the vacuum degree of the high temperature vacuum treatment is 10 -1 ~10 -3 Pa.

[0017] Preferably, the sintering temperature of the high temperature and high pressure sintering in step (3) is 1300-1700° C., the sintering pressure is 4-6 GPa, and the sintering time is 5-20 min.

[0018] The present invention also provides a chromium-zirconium-tungsten compound carbide toughened WC-Co cemented carbide prepared by the preparation method described in the above technical solution, comprising chromium-zirconium-tungsten compound carbide, WC and Co.

[0019] The present invention provides a method for preparing a chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide, comprising the following steps: (1) 2 O 3 、ZrO 2 , WO 3The powder and carbon black powder are ball-milled and mixed, and then vacuum hot carbon reduction is performed to obtain a compound carbide; (2) the compound carbide obtained in step (1) is ball-milled and mixed with WC powder and Co to obtain a mixture; (3) the mixed powder obtained in step (2) is sintered at high temperature and high pressure to obtain a chromium-zirconium-tungsten compound carbide toughened WC-Co cemented carbide. 2 O 3 、ZrO 2 and WO 3 The reduction reaction with carbon black forms a compound carbide, which can refine the grains to increase the dislocation density, thereby increasing the hardness of the material; at the same time, the mixture of compound carbide, WC powder and Co is sintered at high temperature and high pressure to promote the ZrC, Cr 3 C 2 Dispersion and solid-state reaction between different carbides of WC, ZrC, Cr 3 C 2 The Zr, Cr and W atoms in WC move in the lattice through diffusion, find new positions and combine with the surrounding C atoms through covalent bonds to form stable complex carbides, further improving the mechanical properties of the material; shortening the time of grain growth, further refining the grain size; and high temperature and high pressure sintering can limit the continuous growth of grains and inhibit the growth of grains, so that the obtained WC-Co cemented carbide has high hardness, high strength and high toughness. The results of the embodiment show that the Vickers hardness of the WC-Co cemented carbide prepared by the preparation method provided by the present invention is 1885~1925HV, and the fracture toughness is 13.8~14.2MPa·m 1 / 2 . DETAILED DESCRIPTION

[0020] The present invention provides a method for preparing a chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide, comprising the following steps:

[0021] (1) Cr 2 O 3 、ZrO 2 , WO 3 After ball milling with carbon black, vacuum hot carbon reduction is performed to obtain a complex carbide;

[0022] (2) ball-milling the complex carbide obtained in step (1) with WC and Co to obtain a mixture;

[0023] (3) The mixture obtained in step (2) is subjected to high temperature and high pressure sintering to obtain chromium-zirconium-tungsten composite carbide-reinforced WC-Co cemented carbide.

[0024] The present invention converts Cr 2 O 3 、ZrO 2 , WO3 After mixing with carbon black by ball milling, vacuum hot carbon reduction is carried out to obtain a complex carbide.

[0025] In the present invention, the Cr 2 O 3 、ZrO 2 , WO 3 The amount ratio of the substance of carbon black is preferably 1: (0.3-3): (0.1-3): (0.3-1), more preferably 1: (1-2.5): (0.5-2): (0.5-0.9), and most preferably 1: (1.5-2): (1-1.8): (0.6-0.8), which can be specifically 1: 0.67: 0.2: 0.35, 1: 0.4: 0.156: 0.31. In the present invention, by limiting the amount ratio of the reaction raw materials, the content of each carbide in the cemented carbide is controlled, and Cr is achieved at the same time. 2 O 3 、ZrO 2 , WO 3 The sufficient reaction with carbon black can further refine the grains to increase the dislocation density and further improve the hardness of the material.

[0026] In the present invention, the Cr 2 O 3 、ZrO 2 , WO 3 The speed of ball milling and mixing with carbon black is preferably 800-1200 r / min, more preferably 800-1100 r / min, and most preferably 850-900 r / min; the time of ball milling and mixing is preferably 2-5 h, more preferably 2-4 h, and most preferably 2.5-3 h; the ball-to-material ratio of ball milling and mixing is preferably (1-6):1, most preferably (2-5):1, and most preferably (3-4):1. In the present invention, by limiting Cr 2 O 3 、ZrO 2 , WO 3 The process parameters of the ball milling mixing process with carbon black can further suppress the abnormal growth of WC grains in the alloy, promote grain refinement, increase dislocation density, and improve the hardness of WC-Co cemented carbide.

[0027] In the present invention, the temperature of the vacuum hot carbon reduction is preferably 1400-1600°C, more preferably 1400-1550°C, and most preferably 1450-1500°C; the time of the vacuum hot carbon reduction is preferably 1-5h, more preferably 2-4h, and most preferably 3-3.5h; the vacuum degree of the vacuum hot carbon reduction is preferably 10 -1 ~10 -3 Pa, more preferably 10 -2 ~10 -3In the present invention, by optimizing the process parameters of the vacuum thermal carbon reduction reaction, the reaction between the reaction raw materials is promoted, the corresponding carbides can be completely obtained, and the ZrC, Cr 3 C 2 Premixing with WC ensures that ZrC and Cr 3 C 2 The refinement of WC grains further improves the hardness of the alloy.

[0028] Compared with direct mixing of carbides, the compound carbides prepared by the above method can reduce the content of ZrC and Cr. 3 C 2 The density difference between various carbides of WC improves the dispersion uniformity and further realizes the grain refinement, which is beneficial to improve the mechanical properties of cemented carbide.

[0029] In the present invention, the content of WC in the complex carbide is preferably 10 to 30 wt%; 3 C 2 The mass ratio of ZrC and Cr is preferably (0.5-3):1. In the present invention, by limiting the content of each carbide in the composite carbide, the ZrC and Cr 3 C 2 The effect of refining WC grains is beneficial to improving the performance of alloy materials.

[0030] After obtaining the complex carbide, the present invention mixes the complex carbide with WC and Co by ball milling to obtain a mixture.

[0031] In the present invention, the mass ratio of the complex carbide to WC and Co is preferably (0.1-1): (84-94.9): (5-15), more preferably (0.3-0.8): (87-92): (7-13), and most preferably (0.4-6): (88-91): (9-12), which can be specifically 0.6:90:9.4, 0.4:87.6:12. In the present invention, by limiting the mass ratio of the complex carbide to WC and Co, the contents of the hard phase, binder phase and carbide in the cemented carbide are controlled, while promoting the mixing uniformity between the reaction raw materials, avoiding ZrC, Cr 3 C 2 The agglomeration of WC-Co cemented carbide can further improve its toughness and hardness.

[0032] In the present invention, the rotation speed of the ball milling of the compound carbide, WC and Co is preferably 200-500 r / min, more preferably 300-450 r / min, and most preferably 350-400 r / min; the time of the ball milling is preferably 2-12 h, more preferably 5-10 h, and most preferably 7-9 h. The ball-to-material ratio of the ball milling is preferably (3-8):1, more preferably (4-7):1, and most preferably (5-6):1. In the present invention, by limiting the parameters of the ball milling process of the compound carbide, WC and Co, the dispersion uniformity between the compound carbide, WC and Co is further improved, which is beneficial to improving the mechanical properties of the alloy.

[0033] In the present invention, the medium for ball-milling the compound carbide, WC and Co is preferably anhydrous ethanol, and the mass ratio of the material to the volume of the ball-milling medium during the ball-milling is preferably (6-16) g:1 mL, more preferably (8-14) g:1 mL, and most preferably (10-12) g:1 mL. In the present invention, adding anhydrous ethanol can form a thin film on the surface of the ball-milled raw materials to avoid agglomeration between the raw materials and further improve the ball-milling effect.

[0034] The present invention preferably performs drying after the compound carbide is mixed with WC and Co by ball milling; the drying temperature is preferably 80-200°C, more preferably 100-160°C, and most preferably 120-150°C; the drying time is preferably 4-8h, most preferably 5-7h, and most preferably 2.5-6h. In the present invention, by limiting the process parameters of the drying process, the anhydrous ethanol added during the ball milling process is removed, and the influence of the water in the mixture on the subsequent sintering is avoided, so as to further improve the performance of the alloy material.

[0035] After obtaining the mixture, the present invention performs high temperature and high pressure sintering on the obtained mixture to obtain chromium-zirconium-tungsten composite carbide-reinforced WC-Co hard alloy.

[0036] In the present invention, the mixture is preferably subjected to high-temperature vacuum treatment before the high-temperature and high-pressure sintering.

[0037] In the present invention, the temperature of the high temperature vacuum treatment is preferably 800-1200°C, more preferably 900-1100°C, and most preferably 950-100°C; the time of the high temperature vacuum treatment is preferably 1-3h, more preferably 1-2.5h, and most preferably 1.5-2h; the vacuum degree of the high temperature vacuum treatment is preferably 10 -1 ~10 -3 Pa, more preferably 10 -1 ~10 -2Pa. In the present invention, by limiting the process parameters of high-temperature vacuum treatment, the mixture is pretreated so that the mixture is heated evenly, which is conducive to the smooth progress of subsequent rapid sintering, avoids uneven heating of the mixture due to rapid temperature increase, and effectively inhibits the abnormal growth of WC grains, thereby further improving the toughness of WC-Co cemented carbide.

[0038] After the high-temperature vacuum treatment is completed, the present invention preferably performs compression molding on the mixture after the high-temperature vacuum treatment.

[0039] In the present invention, the press forming is preferably cold press forming, and the pressure of the cold press forming is preferably 20 to 100 MPa, more preferably 30 to 60 MPa, and most preferably 40 to 50 MPa. In the present invention, by limiting the pressure of cold press forming, the loose mixture is formed into a green body, laying a foundation for subsequent rapid sintering treatment.

[0040] In the present invention, the sintering temperature of the high temperature and high pressure sintering is preferably 1300-1700°C, more preferably 1400-1600°C, and most preferably 1450-1500°C; the heating rate of the sintering temperature is 20-30°C / s, more preferably 20-25°C / s, and most preferably 20°C / s; the sintering pressure of the high temperature and high pressure sintering is preferably 4-6GPa, more preferably 4-5.5GPa, and most preferably 4.5-5GPa; the sintering time of the high temperature and high pressure sintering is preferably 5-20min, more preferably 8-15min, and most preferably 10-12min; in the present invention, by limiting the process parameters of rapid sintering, it is helpful to densify the alloy material, reduce the generation of pores, and promote the optimization of the microstructure; at the same time, it promotes Cr 3 C 2 The interaction and diffusion of ZrC and WC further refine the grains, inhibit the growth of grains, further improve the toughness of the material, increase the dislocations and grain boundaries inside the alloy, and effectively improve the hardness of the alloy material.

[0041] In the present invention, the green body after high temperature and high pressure sintering is preferably cooled in the furnace to obtain chromium-zirconium-tungsten complex carbide-reinforced WC-Co cemented carbide.

[0042] The preparation method of the present invention comprises preparing Cr 3 C 2 The composite carbides of ZrC and WC are prepared to achieve pre-mixing of different carbides, which can effectively refine the grains to increase the dislocation density, thereby increasing the hardness of the material; at the same time, high temperature and high pressure rapid sintering treatment is adopted to further promote the refinement of the grains, improve the densification of the alloy material, promote the optimization of the microstructure, and improve the strength and toughness of the material, thereby obtaining a WC-Co alloy with high strength, high toughness and high hardness.

[0043] The present invention also provides a chromium-zirconium-tungsten compound carbide toughened WC-Co cemented carbide prepared by the above preparation method, comprising chromium-zirconium-tungsten compound carbide, WC and Co.

[0044] The chromium-zirconium-tungsten composite carbide toughened WC-Co hard alloy provided by the invention has high strength, high toughness and high hardness.

[0045] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] Example 1

[0047] The preparation method of the chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide of this embodiment comprises the following steps:

[0048] (1) 15gCr 2 O 3 Powder, 10gZrO 2 Powder, 3gWO 3 The powder and 5.2 g of carbon black powder were added to a high-energy ball mill and mixed for 2 h, and then vacuum hot carbon reduced at 1500°C for 2 h to obtain a complex carbide; wherein the ball milling speed was 1200 r / min, and the ball-to-material ratio of the ball milling was 6:1;

[0049] (2) 0.6 g of the complex carbide obtained in step (1) was mixed with 90 g of hard phase WC, 9.4 g of binder phase Co and 50 mL of alcohol by ball milling for 3 h, and then dried at 100° C. for 5 h to obtain a mixture; wherein the ball milling speed was 300 r / min, and the ball-to-material ratio of the ball milling was 5:1;

[0050] (3) The mixture obtained in step (2) was heated at 900°C and a vacuum degree of 10 -2 After high-temperature vacuum treatment for 1.5 hours under conditions of 45MPa, the blocks were pressed and assembled into blocks and placed in a six-sided top press. They were sintered at a high temperature and high pressure of 1400°C for 10 minutes at a pressure of 4GPa and a temperature of 4GPa, and cooled with the furnace to obtain chromium-zirconium-tungsten composite carbide reinforced and toughened WC-Co cemented carbide; the heating rate of the sintering temperature was 20°C / s.

[0051] The chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide prepared in this embodiment was tested by indentation method, and the Vickers hardness of the cemented carbide was 1925Hv. The fracture toughness of the cemented carbide was tested by three-point bending test, and the fracture toughness of the cemented carbide was 13.8MPa·m1 / 2 .

[0052] Example 2

[0053] (1) 25gCr 2 O 3 Powder, 10gZrO 2 Powder, 4gWO 3 The powder and 7.7 g of carbon black powder were added into a high-energy ball mill and mixed and ball-milled for 2 h, and then vacuum hot carbon reduced at 1500°C for 2 h to obtain a complex carbide; wherein the ball milling speed was 1200 r / min, and the ball-to-material ratio was 6:1;

[0054] (2) 0.4 g of the complex carbide obtained in step (1) was mixed with 87.6 g of hard phase WC, 12 g of binder phase Co and 50 mL of alcohol, and the mixture was ball-milled for 3 h, and then dried at 100 °C for 5 h to obtain a mixture; wherein the ball milling speed was 300 r / min, and the ball-to-material ratio was 5:1;

[0055] (3) The mixture obtained in step (2) was heated at 900°C and a vacuum degree of 10 -2 After high-temperature vacuum treatment for 1.5 hours under conditions of 45MPa, the products were pressed into shape under the conditions of 45MPa, assembled into blocks and placed in a six-sided top press, and rapidly sintered for 10 minutes at a pressure of 4GPa and a temperature of 1380°C. The products were cooled with the furnace to obtain chromium-zirconium-tungsten composite carbide-reinforced WC-Co cemented carbide; the heating rate of the sintering temperature was 20°C / s.

[0056] The chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide prepared in this embodiment was tested by indentation method, and the Vickers hardness of the cemented carbide was 1885Hv. The fracture toughness of the cemented carbide was tested by three-point bending test, and the fracture toughness of the cemented carbide was 14.2MPa·m 1 / 2 .

[0057] Comparative Example 1

[0058] The difference between Comparative Example 1 and Example 1 is that in step (3), the pressed mixture is placed in a spark plasma sintering system (SPS) for sintering to obtain a cemented carbide material; wherein the sintering pressure is 50 MPa, and the rest is the same as Example 1.

[0059] The chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide prepared in this comparative example was tested by indentation method, and the Vickers hardness of the cemented carbide was 1745Hv. The fracture toughness of the cemented carbide was 11.4MPa·m 1 / 2 .

[0060] Comparative Example 2

[0061] The difference between Comparative Example 2 and Example 2 is that step (1) is omitted, the complex carbide in step (2) is replaced by ZrC, and the rest is the same as Example 1.

[0062] The WC-Co cemented carbide prepared in this comparative example was tested by the indentation method, and the Vickers hardness of the cemented carbide was 1585Hv. The three-point bending test was used to test the cemented carbide, and the fracture toughness of the cemented carbide was 11.2MPa·m 1 / 2 .

[0063] Comparative Example 3

[0064] The difference between Comparative Example 3 and Example 2 is that in step (3), the pressed mixture is placed in SPS for sintering to obtain a cemented carbide material; wherein the sintering pressure is 50 MPa, and the rest is the same as Example 2.

[0065] The chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide prepared in this comparative example was tested by indentation method, and the Vickers hardness of the cemented carbide was 1705Hv. The fracture toughness of the cemented carbide was 13.4MPa·m 1 / 2 .

[0066] In summary, the chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide provided by the present invention has excellent strength and toughness.

[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a chromium-zirconium-tungsten composite carbide toughened WC-Co cemented carbide, comprising the following steps: (1) Cr2O3, ZrO2, WO3 and carbon black are ball-milled and mixed, and then vacuum hot carbon reduction is performed to obtain a complex carbide; (2) ball-milling the complex carbide obtained in step (1) with WC and Co to obtain a mixture; (3) The mixture obtained in step (2) is subjected to high temperature and high pressure sintering to obtain chromium-zirconium-tungsten composite carbide-reinforced WC-Co cemented carbide.

2. The preparation method according to claim 1, characterized in that: The molar ratio of Cr2O3, ZrO2, WO3 and carbon black in the step (1) is 1:(0.3-3):(0.1-3):(0.3-1).

3. The preparation method according to claim 1, characterized in that: The rotation speed of the ball milling mixing in the step (1) is 800-1200 r / min, the time of the ball milling mixing is 2-5 hours, and the ball-to-material ratio of the ball milling mixing is (1-6):

1.

4. The preparation method according to claim 1, characterized in that: The temperature of the vacuum hot carbon reduction in step (1) is 1400-1600° C., the time of the vacuum hot carbon reduction is 1-5 hours, and the vacuum degree of the vacuum hot carbon reduction is 10 -1 ~10 -3 Pa.

5. The preparation method according to claim 1, characterized in that: The mass ratio of the complex carbide to WC and Co in the step (2) is (0.1-1):(84-94.9):(5-15).

6. The preparation method according to claim 1, characterized in that: The rotation speed of the ball milling mixing in the step (2) is 200-500 r / min, the time of the ball milling mixing is 2-12 h, and the ball-to-material ratio of the ball milling mixing is (3-8):

1.

7. The preparation method according to claim 1, characterized in that: The mixture obtained in step (2) is subjected to high-temperature vacuum treatment before the high-temperature and high-pressure sintering in step (3).

8. The preparation method according to claim 7, characterized in that: The temperature of the high temperature vacuum treatment is 800-1200°C, the time of the high temperature vacuum treatment is 1-3 hours, and the vacuum degree of the high temperature vacuum treatment is 10 -1 ~10 - 3 Pa.

9. The preparation method according to claim 1, characterized in that: The sintering temperature of the high temperature and high pressure sintering in the step (3) is 1300-1700° C., the sintering pressure is 4-6 GPa, and the sintering time is 5-20 min.

10. The chromium-zirconium-tungsten complex carbide toughened WC-Co cemented carbide prepared by the preparation method according to any one of claims 1 to 9, comprising chromium-zirconium-tungsten complex carbide, WC and Co.