Repair welding process for backboard containing water channel

By controlling energy, penetration, and welding speed through electron beam welding technology, the problems of target overheating in magnetron sputtering and porosity defects in friction stir welding have been solved, achieving high-quality backplate repair welding results.

CN118926665APending Publication Date: 2024-11-12PIONEER FILM MATERIALS (ANHUI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197799.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During magnetron sputtering, the breakdown or grain formation caused by local overheating of the target material, as well as the defects such as pores or cracks in the water channel processing during friction stir welding, are difficult to repair effectively, especially the repair difficulties caused by equipment size limitations when repairing backplates.

Method used

Electron beam welding technology is used to precisely repair porosity defects by controlling electron beam energy, penetration, focusing and welding speed, thus preventing the back plate from being welded through.

Benefits of technology

It achieves high-quality repair welding results, ensuring that the porosity defects of the back plate are accurately repaired, avoiding the back plate from being welded through, and improving the controllability and quality of the welding depth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926665A_ABST
    Figure CN118926665A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of repair welding processes, and discloses a water-channel-containing back plate repair welding process which comprises the following steps that (1) the face where a welding seam of a back plate is located is sequentially polished, cleaned and dried; (2) in a vacuum environment, electron beam welding is carried out on the pore defects of the weld joint part of the back plate by adopting an electron beam current of 20 mA to 30 mA, an acceleration voltage of 70 kV to 80 kV, a focusing current of 330 mA to 340 mA and a welding speed of 400 mm / min to 500 mm / min; and (3) the backboard is taken out, and air tightness detection is carried out. According to the method, electron beam welding is adopted for repair welding, by controlling electron beam energy, penetration, focusing and welding speed, the welding depth is controllable, the welding quality is high, the pore defect can be accurately repaired, and the backboard can be prevented from being thoroughly welded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of repair welding technology, and in particular to a repair welding technology for a back plate containing a water channel. Background Art

[0002] Magnetron sputtering is a technology that uses a magnetic field to control the release of atoms on the surface of a metal target. During the magnetron sputtering process, the metal target is placed in a vacuum chamber, and the metal atoms on the surface of the target are released by heating or electron bombardment. Then, the magnetic field is used to control the deposition of these metal atoms on the surface of the substrate to form a thin film or coating. Magnetron sputtering technology has the advantages of high film formation rate, good film formation uniformity, and high film quality. It is widely used in optical coatings, conductive films, anti-corrosion coatings and other fields.

[0003] However, long-term magnetron sputtering of high-energy particles can cause local overheating of the target material. If it is not cooled in time, it is easy to cause local breakdown or graining of the sputtering target material. On the one hand, the back plate plays the role of supporting the target material and assembling the machine. On the other hand, a water channel is designed on the back plate, and circulating water is passed through the water channel to cool the target blank.

[0004] The processing of water channels usually requires processing grooves on the back plate, and then welding the cover plate to the grooves by stir friction welding to form water channels on the back plate. However, in stir friction welding, due to parameters, materials and other issues, pores or cracks are prone to occur. At this time, the defects need to be repaired by welding.

[0005] CN115229324A discloses a method for repairing the weld of a back plate, and the method comprises the following steps: (1) using a clamp to fix both ends of the back plate, and performing stir friction welding on the weld of the back plate, during which the clamp and the back plate rotate synchronously, and the stirring head is fixed; (2) after the stir friction welding is completed, the clamp at one end of the back plate is removed, and the stirring head is withdrawn perpendicular to the weld direction of the back plate. During the stir friction welding process, the clamp and the back plate rotate synchronously, and the stirring head is fixed, so that a dense welding structure is formed at the weld of the back plate, and the stirring head is withdrawn perpendicular to the weld direction of the back plate, so as to avoid the hole generated when the stirring needle withdraws from the welding surface.

[0006] The above technical solution uses stir friction welding for repair welding. Although it avoids the problems of pores, cracks, joint deformation and softening of the back plate during traditional fusion welding repair welding, it is limited by the size of the equipment. When repairing the pores in the weld, it is necessary to melt away a large area of ​​metal material around the pores. Therefore, for the repair welding of the back plate, an electron beam welding method is required. Summary of the invention

[0007] The purpose of the present invention is to solve the above-mentioned problems and provide a repair welding process for a back plate containing a water channel. The repair welding process adopts electron beam welding for repair welding. By controlling the electron beam energy, penetration, focusing and welding speed, the welding depth is controllable and the welding quality is high. The porosity defects can be accurately repaired and the back plate can be prevented from being welded through.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A back plate repair welding process containing water channels comprises the following steps:

[0010] Step (1): grinding, cleaning and drying the weld surface of the back plate in sequence;

[0011] Step (2): in a vacuum environment, electron beam welding is performed on the porosity defects at the weld of the back plate using an electron beam current of 20 mA to 30 mA, an acceleration voltage of 70 to 80 kV, a focusing current of 330 to 340 mA, and a welding speed of 400 mm / min to 500 mm / min;

[0012] Step (3): Take out the back panel and perform an airtightness test.

[0013] Wherein, in step (2), the electron beam current can be 20mA, 21mA, 22mA, 23mA, 24mA, 25mA, 26mA, 27mA, 28mA, 29mA, 30mA, but is not limited to the listed values, and other values ​​not listed within this numerical range are applicable;

[0014] The accelerating voltage may be 71 kV, 72 kV, 73 kV, 74 kV, 75 kV, 76 kV, 77 kV, 78 kV, 79 kV, 80 kV, but is not limited to the listed values, and other values ​​not listed within this numerical range are applicable;

[0015] The focusing current can be 330mA, 331mA, 332mA, 333mA, 334mA, 335mA, 336mA, 337mA, 338mA, 339mA, 340mA, but is not limited to the listed values, and other values ​​not listed within this numerical range are applicable;

[0016] The welding speed can be 400mm / min, 410mm / min, 420mm / min, 430mm / min, 440mm / min, 450mm / min, 460mm / min, 470mm / min, 480mm / min, 490mm / min, 500mm / min, but is not limited to the listed values. Other values ​​not listed in this numerical range are applicable;

[0017] Preferably, in the step (1), during grinding, the height of the back plate is processed to be 0.2-0.3 mm greater than the height of the finished product, and can be 0.2 mm, 0.21 mm, 0.22 mm, 0.23 mm, 0.24 mm, 0.25 mm, 0.26 mm, 0.27 mm, 0.28 mm, 0.29 mm, 0.3 mm.

[0018] In the step (2), an electron beam welding machine is used to provide a vacuum environment and perform electron beam welding on the back plate. The electron beam is focused on the surface of the back plate, and the vacuum degree is 1×10 -3 ~1×10 -2 Pa.

[0019] The model of the electron beam welding equipment used is Guilin Shida THDW-12. The vacuum degree can be 1×10 -3 Pa, 2×10 -3 Pa, 3×10 -3 Pa, 4×10 -3 Pa, 5×10 -3 Pa, 6×10 -3 Pa, 7×10 -3 Pa, 8×10 -3 Pa, 9×10 -3 Pa, 1×10 -12 Pa.

[0020] Preferably, in step (3), before the air tightness test, the back panel is first polished to the finished size and cleaned until there are no welding marks on the surface.

[0021] Specifically, if the air tightness test is performed before polishing, the air tightness test may pass, but air holes may appear after polishing. Therefore, in order to avoid such a problem, the back panel needs to be polished to the finished size first, and then the air tightness test can be performed.

[0022] Preferably, in step (1) and step (3), anhydrous ethanol or isopropanol is used for cleaning. Anhydrous ethanol and isopropanol belong to anhydrous alcohol solvents, which can effectively remove impurities such as dirt and grease, and have a good cleaning effect. In addition, anhydrous ethanol and isopropanol have good volatility. The residual solvent after cleaning will evaporate naturally without leaving water stains or residues.

[0023] Preferably, in step (3), the polishing is performed by using a pneumatic polishing machine, and the model of the pneumatic polishing machine used is: Bodun BD-0125.

[0024] Preferably, the air tightness detection is performed using a helium mass spectrometer leak detector. Helium is a rare gas with extremely small molecules that can easily pass through tiny pores or holes. Therefore, when helium is used for air tightness detection, tiny air leaks can be detected more easily, and even extremely tiny leaks can be accurately detected. Moreover, it will not cause harm to operators or pollution to the environment. The model of the helium mass spectrometer leak detector used is: Wanyi SFJ-231D.

[0025] Preferably, the backplane is a TU1 oxygen-free copper backplane, which meets the (GB / T 5231-2001) standard.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention adopts electron beam welding for repair welding. By controlling the electron beam energy, penetration, focusing and welding speed, the welding depth is controllable and the welding quality is high. The porosity defects can be accurately repaired and the back plate can be prevented from being welded through. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a schematic diagram of the back plate of the present invention after welding;

[0029] Figure 2 It is a schematic diagram of a qualified back plate after polishing of the present invention;

[0030] Figure 3 is a schematic diagram of a back plate of the present invention being welded through;

[0031] Figure 4 It is a schematic diagram of pores appearing after the back plate of the present invention is polished. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Before presenting the embodiments and comparative examples of the present invention, it should be noted that the semi-finished backplane used in the following embodiments and comparative examples is a TU1 oxygen-free copper backplane, which meets the (GB / T 5231-2001) standard and has the following dimensions: diameter 104.8 mm, height 40.5 mm, water channel width 11 mm, water channel depth 6.2 mm; the dimensions of the finished backplane are: diameter 100 mm, height 39 mm, water channel width 11 mm, water channel depth 6.2 mm.

[0034] Example 1

[0035] A back plate repair welding process containing water channels comprises the following steps:

[0036] Step (1): grinding the surface of the weld of the TU1 oxygen-free copper back plate, processing the height of the TU1 oxygen-free copper back plate to be 0.2 mm greater than the finished product height, then cleaning and completely drying;

[0037] Step (2): Place TU1 oxygen-free copper in an electron beam welding device and evacuate to a vacuum degree of 1×10 -2 Pa, electron beam welding was performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 70 kV, a focusing current of 330 mA, and a welding speed of 400 mm / min;

[0038] Step (3): Take out the backplane and perform air tightness test on the TU1 oxygen-free copper backplane.

[0039] Example 2

[0040] The method is basically the same as Example 1, except that, in step (3), before the air tightness test, the back panel is first polished to the finished size using a pneumatic polishing machine and cleaned until there is no welding mark on the surface.

[0041] Example 3

[0042] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 30 mA, an acceleration voltage of 80 kV, a focusing current of 340 mA, and a welding speed of 500 mm / min.

[0043] Example 4

[0044] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 80 kV, a focusing current of 330 mA, and a welding speed of 500 mm / min.

[0045] Example 5

[0046] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 30 mA, an acceleration voltage of 70 kV, a focusing current of 340 mA, and a welding speed of 500 mm / min.

[0047] Example 6

[0048] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 25 mA, an acceleration voltage of 75 kV, a focusing current of 335 mA, and a welding speed of 450 mm / min.

[0049] Example 7

[0050] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 80 kV, a focusing current of 340 mA, and a welding speed of 400 mm / min.

[0051] Example 8

[0052] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 30 mA, an acceleration voltage of 70 kV, a focusing current of 330 mA, and a welding speed of 400 mm / min.

[0053] Example 9

[0054] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 25 mA, an acceleration voltage of 80 kV, a focusing current of 340 mA, and a welding speed of 500 mm / min.

[0055] Example 10

[0056] It is basically the same as Example 2, except that in step (1), the height of the TU1 oxygen-free copper backplane is processed to be 0.3 mm greater than the finished product height.

[0057] Embodiment 11

[0058] It is basically the same as Example 2, except that in step (1), the height of the TU1 oxygen-free copper backplane is processed to be 0.1 mm greater than the finished product height.

[0059] Example 12

[0060] It is basically the same as Example 2, except that in step (1), the height of the TU1 oxygen-free copper backplane is processed to be 0.4 mm greater than the finished product height.

[0061] Example 13

[0062] It is basically the same as Example 2, except that the back plate used is an aluminum alloy back plate.

[0063] Comparative Example 1

[0064] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 10 mA, an acceleration voltage of 70 kV, a focusing current of 330 mA, and a welding speed of 400 mm / min.

[0065] Comparative Example 2

[0066] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 40 mA, an acceleration voltage of 70 kV, a focusing current of 330 mA, and a welding speed of 400 mm / min.

[0067] Comparative Example 3

[0068] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 70 kV, a focusing current of 330 mA, and a welding speed of 350 mm / min.

[0069] Comparative Example 4

[0070] The method is basically the same as Example 2, except that, in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 70 kV, a focusing current of 330 mA, and a welding speed of 550 mm / min.

[0071] Comparative Example 5

[0072] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 60 kV, a focusing current of 330 mA, and a welding speed of 400 mm / min.

[0073] Comparative Example 6

[0074] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 90 kV, a focusing current of 330 mA, and a welding speed of 400 mm / min.

[0075] Comparative Example 7

[0076] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 70 kV, a focusing current of 320 mA, and a welding speed of 400 mm / min.

[0077] Comparative Example 8

[0078] The method is basically the same as Example 2, except that in step (2), electron beam welding is performed on the porosity defects in the weld with an electron beam current of 20 mA, an acceleration voltage of 70 kV, a focusing current of 350 mA, and a welding speed of 400 mm / min.

[0079] The repair welding processes of the back plate containing water channels of Examples 1 to 13 and Comparative Examples 1 to 8 were respectively used to repair the porosity defects on the back plate welds. The repair welding results are shown in Table 1:

[0080] Table 1 Repair welding results of back plate with water channel

[0081]

[0082]

[0083] Among them, the backplane is qualified if, after being processed to the finished size, there are no weld marks on the surface of the backplane and it can pass the airtightness test.

[0084] The operator can judge whether the back of the back plate is welded through by visual observation.

[0085] Result analysis:

[0086] 1. From the results of Examples 1 to 9, it can be concluded that when the electron beam current is set at 20 to 30 mA, the acceleration voltage is set at 70 to 80 kV, the welding speed is set at 400 to 500 mm / min, and the focusing current is set at 330 to 340 mA, the repair welding effect is most ideal, and the results are all qualified backplanes. Although Example 1 is qualified and passes the airtightness test, the weld is obvious because it has not been subsequently polished. After polishing, there is no weld mark on the surface of Examples 2 to 9. The results are as follows Figure 1 and Figure 2 As shown, it means that under this welding parameter, there will be no pores after grinding and the weld penetration is ideal.

[0087] 2. From the results of Example 2 and Example 10, it can be seen that under the electron beam current of 20mA, the acceleration voltage of 70kV, the welding speed of 400mm / min, and the focusing current of 330mA, there is not much difference in the results of processing the height of the back plate to 0.3mm and 0.2mm greater than the height of the finished product, indicating that under the parameters of this electron beam equipment, the back plate height of 0.2 to 0.3mm relative to the finished product can meet the requirements of repair welding. The results are as follows Figure 2 shown.

[0088] 3. From the results of Example 2, Example 11, and Example 12, it can be seen that the back plate of Example 2 is polished to 0.2 mm higher than the finished product, while the back plate of Example 11 is polished to 0.1 mm higher than the finished product, and the back plate of Example 12 is polished to 0.4 mm higher than the finished product. Both Example 11 and Example 12 exceed the range of 0.2 to 0.3 mm. From the results, it can be seen that due to the excessive thickness of Example 12, after the repair welding is completed and then polished, the weld of the repair welding will also be polished away, resulting in the reappearance of pores. The results refer to Figure 4However, due to the low thickness and insufficient grinding allowance of Example 11, the weld is still obvious after being ground to the finished product size. Figure 1 .

[0089] 4. From the results of Example 2 and Example 13, it can be seen that Example 13 uses an aluminum alloy back plate and adopts the same welding parameters as Example 2. The welding parameters are too large for welding the aluminum back plate. This shows that the parameters of the present invention are more suitable for the back plate made of TU1 oxygen-free copper. Figure 3 .

[0090] 5. From the results of Example 2, Example 5, Comparative Example 1, and Comparative Example 2, it can be seen that under the same acceleration voltage, welding speed, and grinding height, Comparative Example 1 and Comparative Example 2 both exceed the electron beam current range of 20 to 30 mA. From the results of Comparative Example 1, it can be concluded that when the welding current is too small, the total welding heat input is too small, and the metal around the weld cannot be well melted, resulting in residual pore defects on the surface of the back plate after being processed to the finished product size. The results refer to Figure 4 From the results of comparative example 2, it can be concluded that when the welding current is too large, the total welding heat input is too large, which will cause the back of the back plate to be welded through, that is, the air tightness of the water channel inside the back plate is destroyed. Figure 3 , which is also an unqualified product.

[0091] 6. From the results of Example 2, Example 5, Comparative Example 3, and Comparative Example 4, it can be seen that the welding speed is also related to the heat input of welding. Under the same electron beam current, acceleration voltage, focusing current, and grinding height, the welding speed is lower than the range of 400-500 mm / min, indicating that the welding speed is smaller. Therefore, the longer the electron beam stays in the weld, the greater the heat input, resulting in the back of the back plate being welded through, that is, Comparative Example 3. The results refer to Figure 3 Comparative Example 4 uses a welding speed higher than 400-500 mm / min. Therefore, the shorter the time the electron beam stays on the weld, the smaller the heat input, resulting in failure to melt the metal around the weld well. Therefore, after being processed to the finished product size, porosity defects appeared in Comparative Example 4. Figure 4 .

[0092] 7. From the results of Example 2, Example 5, Comparative Example 5, and Comparative Example 6, it can be seen that under the same electron beam current, welding speed, and grinding height, Comparative Examples 5 and 6 both exceed the acceleration voltage range of 70 to 80 kV. From the results of Comparative Examples 5 and 6, it can be concluded that the electron beam current and the acceleration voltage jointly affect the heat input of welding. Therefore, when the electron beam current is lower than the range of 70 to 80 kV, the total welding heat input is too small, that is, the results of Comparative Example 5 refer to Figure 4When the electron beam current is higher than 70-80 kV, the total welding heat input is too small, that is, the result of Example 6 is referenced Figure 3 .

[0093] 8. From the results of Example 2, Example 5, Comparative Example 7 and Comparative Example 8, it can be seen that Comparative Example 7 uses a focusing current range lower than 330-340 mA. Too small a focusing current will lead to insufficient heat input during welding, resulting in insufficient welding depth, so the pores reappear after grinding. The results are as follows Figure 4 As shown; however, too large a focusing current will result in too high a heat input, causing the material to overheat, burn through, or serious excessive penetration, that is, the back plate is welded through, with the result as shown Figure 3 shown.

[0094] In summary, the present invention adopts electron beam welding for repair welding. By controlling the electron beam current, acceleration voltage, focusing current and welding speed, the welding depth is controllable and the welding quality is high. The porosity defects can be accurately repaired and the back plate can be prevented from being welded through. Experiments have shown that the back plate is polished to 0.2-0.3 mm higher than the finished product size, and the electron beam current is controlled at 20-30 mA, the acceleration voltage is controlled at 70-80 kV, the welding speed is controlled at 400-500 mm / min, and the focusing current is controlled at 330-340 mA to achieve the most ideal repair welding result. Experiments have also shown that the present invention is more suitable for a back plate made of TU1 oxygen-free copper.

[0095] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements or modifications without departing from the principle of the present invention. These improvements or modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A back plate repair welding process containing water channel, characterized in that: The steps include: Step (1): grinding, cleaning and drying the weld surface of the back plate in sequence; Step (2): in a vacuum environment, electron beam welding is performed on the porosity defects at the weld of the back plate using an electron beam current of 20 mA to 30 mA, an acceleration voltage of 70 to 80 kV, a focusing current of 330 to 340 mA, and a welding speed of 400 mm / min to 500 mm / min; Step (3): Take out the back panel and perform an airtightness test.

2. The water channel back plate repair welding process according to claim 1 is characterized in that: In the step (1), during grinding, the height of the back plate is processed to be 0.2 to 0.3 mm greater than the height of the finished product.

3. The water channel back plate repair welding process according to claim 1 is characterized in that: In the step (2), an electron beam welding machine is used to provide a vacuum environment and perform electron beam welding on the back plate. The electron beam is focused on the surface of the back plate, and the vacuum degree is 1×10 -3 ~1×10 -2 Pa.

4. The water channel back plate repair welding process according to claim 1 is characterized in that: In the step (3), before the air tightness test, the back plate is first polished to the finished size and cleaned until there are no welding marks on the surface.

5. The repair welding process for the back plate containing water channel according to claim 4 is characterized in that: In the steps (1) and (3), anhydrous ethanol or isopropanol is used for cleaning.

6. The repair welding process for the back plate containing water channel according to claim 4 is characterized in that: In the step (3), the polishing is performed using a pneumatic polishing machine.

7. The repair welding process for the back plate containing water channel according to claim 1 is characterized in that: The air tightness detection is performed using a helium mass spectrometer leak detector.

8. The water channel back plate repair welding process according to claim 1 is characterized in that: The backplane is a TU1 oxygen-free copper backplane.