High-toughness automobile color changing film and preparation method thereof
By using the fusion stacking technology of carbon crystal wear-resistant layer, TPH material repair coating, rebound toughness layer and TPU electrostatic layer in the automotive color change film, the problem of insufficient toughness of the color change film is solved, and a more robust and tough automobile is achieved Color-changing film extends service life and reduces maintenance costs.
Patent Information
- Application Number
- CN202410994009.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing automotive color-changing film has poor toughness, which leads to poor toughness and durability during use.
High-strength tough automotive color-changing film prepared by fusion stacking of carbon crystal wear-resistant layer, TPH material repair coating, rebound toughness layer, TPU electrostatic layer and nano intelligent adsorption layer, improve the color-changing film through specific raw material ratios and process steps. toughness.
It significantly improves the toughness and durability of the color change film, can withstand scratches caused by friction from high-hard sharp objects on the surface, extends service life and reduces maintenance and replacement costs.
Smart Images

Figure CN118927752A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of color-changing films, and in particular relates to a high-strength and tough automobile color-changing film and a preparation method thereof. Background Art
[0002] As the new favorite in the car beauty industry, invisible car film has been recognized by many domestic consumers. The number of cars in use and the number of new cars have brought huge potential market space for invisible car film. Car body color-changing film is a service that uses a film with rich and diverse colors to change the appearance of the entire car or part of it by covering and pasting it as a whole. Car body color-changing film is mainly attached to the surface of the car body through polymer materials and is easy to remove.
[0003] In the related prior art, for example, the invention patent authorized by China is entitled as a method for preparing a coating-type color-changing TPU color-changing film, and the authorization announcement number is
[0004] CN114989739B specifically discloses a scheme that "includes the following steps: (1) coating a functional coating on one surface of a TPU film, and baking and curing to obtain a pre-treated film; (2) performing plasma etching on the other surface of the pre-treated film, and then obtaining a surface-modified TPU film; (3) uniformly coating the etched surface of the surface-modified TPU film with a layer of water-based color glue, baking and drying to cure, and adhering a pressure-sensitive adhesive layer to the surface of the water-based color glue layer to obtain a coated TPU color-changing film." This color-changing film pre-processes the TPU film with plasma bias etching to form a nano-scale pattern on the film, and has the firmness of the color glue layer and the effect that the color glue layer is not easy to fall off; however, the toughness of this color-changing film is poor, resulting in the color-changing film still being weak and not durable during use. Summary of the invention
[0005] In view of the above problems existing in the prior art, an object of the present invention is to provide a high-strength and tough automobile color-changing film and a preparation method thereof.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A high-strength and tough car color-changing film, the TPU color-changing film is formed by fusion and stacking of a carbon crystal wear-resistant layer, a TPH material repair coating, a rebound toughness layer, a TPU electrostatic layer and a nano-intelligent adsorption layer from top to bottom; wherein the TPU electrostatic layer is calculated by weight of the following raw materials:
[0008] 30-60 parts of thermoplastic polyurethane resin, 10-38 parts of polyol, 5-12 parts of diisocyanate, 5-10 parts of chain extender and 3-10 parts of static eliminator; The preparation method of TPU thermoplastic polyurethane static layer includes the following steps: the first step, preparing raw materials with quantitative proportion;
[0009] Step 2: Put polyol and diisocyanate into a reaction container, and control the temperature to be in the range of 48-100°C and the reaction time T to be 0.5-2.5h to obtain prepolymer a;
[0010] The third step is to add thermoplastic polyurethane resin, chain extender and static eliminator to the obtained prepolymer a, and control the temperature value range to be 110-150°C and the reaction time T to be 1.5-2h; the generated polymer TPU is mixed, granulated and flattened to form a TPU static layer.
[0011] As a preferred technical solution of the present invention, the TPU electrostatic layer is calculated by weight of the following raw materials:
[0012] 52 parts of thermoplastic polyurethane resin, 26 parts of polyol, 8 parts of diisocyanate, 10 parts of chain extender and 4 parts of static eliminator.
[0013] As a preferred technical solution of the present invention, the TPU electrostatic layer is calculated by weight of the following raw materials:
[0014] 48 parts of thermoplastic polyurethane resin, 27 parts of polyol, 12 parts of diisocyanate, 7 parts of chain extender and 6 parts of static eliminator.
[0015] As a preferred technical solution of the present invention, the hardness of the thermoplastic polyurethane resin is 35A-80A.
[0016] As a preferred technical solution of the present invention, the static eliminator includes one of a higher alcohol sulfate ester salt, an aliphatic sulfonate salt, or a higher alcohol phosphate ester salt.
[0017] The present invention also provides a method for preparing the high-toughness automobile color-changing film as described above, comprising the following steps:
[0018] S1, heating the TPH material repair coating, the rebound toughness layer, the TPU electrostatic layer and the nano smart adsorption layer at 120° C. to fuse and stack the TPH material repair coating, the rebound toughness layer, the TPU electrostatic layer and the nano smart adsorption layer together to obtain a fused stacking layer A;
[0019] S2, compounding the carbon crystal wear-resistant layer on the surface of the fused stacking layer A obtained in step S1 to obtain a composite film B;
[0020] S3. The composite film B obtained in step S2 is allowed to stand at a temperature of 82-95°C for 72-96 hours, then placed in a cooling machine for cooling, and wound up using a winding device to obtain a high-strength and tough automotive color-changing film.
[0021] As a preferred technical solution of the present invention, in step S3, the standing temperature is 90° C. and the standing time T is 90 h.
[0022] The present invention relates to a high-strength and toughness automobile color-changing film and a preparation method thereof, which have the following beneficial effects: the high-strength and toughness automobile color-changing film of the present invention has a TPU electrostatic layer and also contains a TPH material repair coating and a rebound toughness layer, especially the TPH material has the characteristics of high strength and toughness, and is wear-resistant and scratch-resistant, and can resist scratches caused by friction of high-hardness sharp objects on its surface; in addition, a rebound toughness layer is provided, that is, through the provision of multiple toughness structures, the toughness of the automobile color-changing film of the present invention can be further improved, making it more durable and having a long service life, and can reduce the high cost caused by maintenance and replacement.
[0023] The present invention will be further described below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the structure of the high-strength and tough car color-changing film applied for in the present invention.
[0025] Reference numerals - In the drawings:
[0026] a-Carbon crystal wear-resistant layer; b-TPH material repair coating; c-rebound toughness layer; d-TPU electrostatic layer; e-Nano intelligent adsorption layer. DETAILED DESCRIPTION
[0027] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0028] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0029] The high-toughness car color-changing film provided by the present invention is combined with Figure 1 As shown, the TPU color-changing film is formed by the fusion and stacking of a carbon crystal wear-resistant layer a, a TPH material repair coating b, a rebound toughness layer c, a TPU electrostatic layer d, and a nano-intelligent adsorption layer e from top to bottom; wherein the TPU electrostatic layer d is calculated according to the weight of the following raw materials:
[0030] 30-60 parts of thermoplastic polyurethane resin, 10-38 parts of polyol, 5-12 parts of diisocyanate, 5-10 parts of chain extender and 3-10 parts of static eliminator; The preparation method of TPU thermoplastic polyurethane static layer includes the following steps: the first step, preparing raw materials with quantitative proportion;
[0031] Step 2: Put polyol and diisocyanate into a reaction container, and control the temperature to be in the range of 48-100°C and the reaction time T to be 0.5-2.5h to obtain prepolymer a;
[0032] The third step is to add thermoplastic polyurethane resin, chain extender and static eliminator to the obtained prepolymer a, and control the temperature value range to be 110-150°C and the reaction time T to be 1.5-2h; the generated polymer TPU is mixed, granulated and flattened to form a TPU static layer.
[0033] In order to illustrate the present invention, the present invention provides 4 embodiments, 3 comparative examples and 1 test example, wherein the static eliminator in the experiment includes one of a higher alcohol sulfate ester salt, aliphatic sulfonate salt or a higher alcohol phosphate ester salt.
[0034] Example 1
[0035] The preparation of raw materials and the TPU electrostatic layer are calculated according to the weight parts of the following raw materials: 30 parts of thermoplastic polyurethane resin with a hardness of 35A, 38 parts of polyol, 12 parts of diisocyanate, 10 parts of chain extender and 10 parts of static eliminator; the preparation method of the TPU electrostatic layer is shown in the above steps and will not be described in detail here.
[0036] The method for preparing the high-strength and tough automobile color-changing film applied by the present invention is as follows:
[0037] The method comprises the following steps S1, heating the TPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e at 120° C. to fuse and stack the TPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e together to obtain a fused stacking layer A;
[0038] S2, compounding the carbon crystal wear-resistant layer a onto the surface of the fused stacking layer A obtained in step S1 to obtain a composite film B;
[0039] S3. Allow the composite film B obtained in step S2 to stand at 82-95°C for 72-96h, then place it in a cooler for cooling, and use a winding device to wind it up to obtain a high-strength and tough car color-changing film; wherein in step S3, the standing temperature is 90°C and the standing time T is 90h.
[0040] Example 2
[0041] The preparation of raw materials and the TPU electrostatic layer are calculated according to the weight parts of the following raw materials: 52 parts of thermoplastic polyurethane resin with a hardness of 42A, 26 parts of polyol, 8 parts of diisocyanate, 10 parts of chain extender and 4 parts of static eliminator; the preparation method of the TPU electrostatic layer is shown in the above steps and will not be described in detail here.
[0042] The method for preparing the high-strength and tough automobile color-changing film applied by the present invention is as follows:
[0043] The method comprises the following steps S1, heating the TPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e at 120° C. to fuse and stack the TPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e together to obtain a fused stacking layer A;
[0044] S2, compounding the carbon crystal wear-resistant layer a onto the surface of the fused stacking layer A obtained in step S1 to obtain a composite film B;
[0045] S3. Allow the composite film B obtained in step S2 to stand at 82-95°C for 72-96h, then place it in a cooler for cooling, and use a winding device to wind it up to obtain a high-strength and tough car color-changing film; wherein in step S3, the standing temperature is 90°C and the standing time T is 90h.
[0046] Example 3
[0047] The preparation of raw materials and the TPU electrostatic layer are calculated according to the weight parts of the following raw materials: 48 parts of thermoplastic polyurethane resin with a hardness of 75A, 27 parts of polyol, 12 parts of diisocyanate, 7 parts of chain extender and 6 parts of static eliminator; the preparation method of the TPU electrostatic layer is shown in the above steps and will not be described in detail here.
[0048] The method for preparing the high-strength and tough automobile color-changing film applied by the present invention is as follows:
[0049] The method comprises the following steps S1, heating the TTPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e at 120° C. to fuse and stack the TPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e together to obtain a fused stacking layer A;
[0050] S2, compounding the carbon crystal wear-resistant layer a onto the surface of the fused stacking layer A obtained in step S1 to obtain a composite film B;
[0051] S3. Allow the composite film B obtained in step S2 to stand at 82-95°C for 72-96h, then place it in a cooler for cooling, and use a winding device to wind it up to obtain a high-strength and tough car color-changing film; wherein in step S3, the standing temperature is 90°C and the standing time T is 90h.
[0052] Example 4
[0053] Preparation of raw materials: TPU electrostatic layer is calculated according to the weight parts of the following raw materials:
[0054] 60 parts of thermoplastic polyurethane resin with a hardness of 80A, 27 parts of polyol, 5 parts of diisocyanate, 5 parts of chain extender and 3 parts of static eliminator; the preparation method of the TPU static layer is shown in the above steps and will not be described in detail here.
[0055] The method for preparing the high-strength and tough automobile color-changing film applied by the present invention is as follows:
[0056] The method comprises the following steps S1, heating the TPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e at 120° C. to fuse and stack the TPH material repair coating b, the rebound toughness layer c, the TPU electrostatic layer d and the nano intelligent adsorption layer e together to obtain a fused stacking layer A;
[0057] S2, compounding the carbon crystal wear-resistant layer a onto the surface of the fused stacking layer A obtained in step S1 to obtain a composite film B;
[0058] S3. Allow the composite film B obtained in step S2 to stand at 82-95°C for 72-96h, then place it in a cooler for cooling, and use a winding device to wind it up to obtain a high-strength and tough car color-changing film; wherein in step S3, the standing temperature is 90°C and the standing time T is 90h.
[0059] Comparative Example 1
[0060] Different from Example 1, no TPU electrostatic layer d is provided during the preparation.
[0061] Comparative Example 2
[0062] Different from Example 1, no TPH material repair coating b is provided during the preparation.
[0063] Comparative Example 3
[0064] Different from Example 1, no rebound toughness layer c is provided during the preparation.
[0065] Test example
[0066] Different from Example 1, the TPH material repair coating, rebound toughness layer and TPU electrostatic layer are not provided at the same time during the preparation.
[0067] According to the test standards, a variety of color-changing films obtained from Examples 1-4, Comparative Examples 1-3 and Test Examples of the present invention are specifically selected for performance testing. The test items include scratch testing, tensile testing and impact testing, as shown below.
[0068] 1. Scratch test
[0069] The scratch test is to evaluate the toughness of the color-changing film based on the degree of deformation after the surface is scratched. The test steps are as follows:
[0070] (1) Use a pencil or similar tool to make a scratch on the surface with a length of 8 mm and a depth of 1 mm;
[0071] (2) Observe the scratches on the color-changing film with the naked eye or a microscope (the present invention adopts visual observation). If cracks appear at the scratches on the color-changing film, it indicates that the toughness is poor; otherwise, it indicates that the toughness is good. The test results of each embodiment, comparative example and test example are recorded in Table 1.
[0072] project Are there any cracks in the scratches? Excellent toughness Example 1 No excellent Example 2 No excellent Example 3 No excellent Example 4 No excellent Comparative Example 1 have Difference Comparative Example 2 have Difference Comparative Example 3 No / Test example have Difference
[0073] It can be seen from Table 1 above that: Examples 1-4 had no cracks, while Comparative Examples 1-3 and the test example had cracks. The result of Comparative Example 3 may be due to errors in the test operation or errors in naked eye observation, which can explain that the color-changing films obtained in Examples 1-4 have better toughness; therefore, the color-changing film obtained by the present invention has better high strength and toughness characteristics.
[0074] 2. Tensile test
[0075] The tensile test is to test the toughness of the color-changing film by applying tensile force; the test steps are as follows:
[0076] (1) Fix the color-changing film on a stretching machine and gradually apply tension from both ends;
[0077] (2) When the color-changing film breaks, record the value of the tensile force and calculate the tensile elongation of the color-changing film;
[0078] (3) The higher the tensile elongation, the better the toughness, and vice versa. The test results of each embodiment, comparative example and test example are recorded in Table 2.
[0079] project Is there a break? Tension(N) Tensile elongation (%) Example 1 no 31.2 502 Example 2 no 40.5 701 Example 3 no 41.6 713 Example 4 no 38.1 623 Comparative Example 1 yes 21.2 289 Comparative Example 2 yes 23.8 455 Comparative Example 3 yes 22.6 401 Test example yes 18.1 103
[0080] It can be seen from Table 2 above that the tensile elongation of Examples 1-4 is greater than that of the comparative example and the test example, indicating that the color-changing films obtained in Examples 1-4 have significantly improved tensile elongation performance; when the rebound toughness layer c is not set in Comparative Example 3, the toughness performance of the color-changing film is slightly inferior to that of the color-changing film of Comparative Example 2; the tensile force and tensile elongation of the samples are tested in accordance with GB / T13022-1991 Test Method for Tensile Properties of Plastic Films, and the tensile force is ≥28N, which meets the industry standard for car cover films and is rated as good; the tensile force is <28N, which does not meet the industry standard for car cover films and is rated as poor; the tensile elongation is ≥500%, and the performance is good; the tensile elongation is <500%, and the performance is poor; the higher the tensile elongation, the better the toughness, and it can be seen that the tensile elongation performance of Examples 2 and 3 is better; therefore, the color-changing film obtained by the present invention has better high strength and toughness characteristics.
[0081] The above-mentioned stretching machine adopts a microcomputer-controlled electronic universal tensile testing machine produced by Liboshi Company.
[0082] 3. Impact test
[0083] The impact test is to test the toughness of the color-changing film by applying impact force. The impact tester used is the test product sold by Shanzhi Instrument Co., Ltd. The test steps are as follows:
[0084] (1) Using an impact tester, place the color-changing film on a bracket;
[0085] (2) then applying an impact force to the color-changing film and recording the maximum impact value;
[0086] (3) The larger the impact value, the better the toughness, and vice versa. The test results of various embodiments, comparative examples and test examples are recorded in Table 3.
[0087] project Maximum shock value (N) Example 1 39.6 Example 2 42 Example 3 41.8 Example 4 40.1 Comparative Example 1 18.9 Comparative Example 2 21.3 Comparative Example 3 20.8 Test example 9.8
[0088] From the data recorded in the above Table 3, it can be seen that: the maximum impact values of Examples 1-4 are all greater than those of the comparative examples and the test examples, indicating that the color-changing films obtained in Examples 1-4 have significantly improved maximum impact value performance; in summary, Tables 1 / 2 and 3 above: the color-changing films obtained by the present invention have excellent high strength and toughness characteristics, and are wear-resistant and scratch-resistant, and can resist scratches caused by friction of high-hardness sharp objects on their surface; in addition, a rebound toughness layer is provided, that is, through the setting of multiple tough structures, the toughness of the car color-changing film of the present invention can be further improved, making it more durable and having a long service life, which can reduce the high cost of maintenance and replacement.
[0089] During the above test, the test product is placed on the table of the impact tester, and a steel ball of a specified weight is dropped freely from a specified drop height onto the product to impact the product, and then the product appearance and various performances are checked; the impact tester is based on GB / T9962-1998 Safety glass materials for building - Safety glass performance specifications and test methods
[0090] The impact tester is designed according to the "6.10 Drop Ball Impact Peeling Performance Method" to meet the impact test requirements for building safety interlayers. The reliability test standards of the impact tester are: JIS R3205:1989, ISO / DIS125421 12543-6:1997AS / NZS2208:1996, GB / T9962-1999.
[0091] The technical parameters of the impact tester mentioned above include: 1. Steel ball weight: 55, 64g, 110, 225, 535g (select a steel ball order note) can be purchased according to requirements); 2. Permissible error of steel ball weight: ±5g; 3. Protection device: there are protective net boxes around; 4. Control and lifting method: circuit control electromagnet suction cup, manual lifting electromagnet fixing rod; 5. Drop height: 0~1500 / 2000mm (2 meters need to be customized) (manual, steel ruler display scale, according to requirements 1. Drop height display: scale steel ruler plus right-angle ruler vertical indication; 2. Drop height accuracy: 1mm; 3. Drop rod shape: square rod; 4. Sample frame working space: 400×350mm; 5. Sample clamping method: clamp clamping; 6. Drop iron plate: thickness 10mm; 7. Machine size (L×W×H): about 500×400×1800mm; 8. Machine weight: 30kg; 9. Working power supply: AC220V, 50HZ.
[0092] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0093] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A high-strength and tough car color-changing film, characterized in that: The TPU color-changing film is stacked from top to bottom by a carbon crystal wear-resistant layer, a TPH material repair coating, a rebound toughness layer, a TPU electrostatic layer, and a nano-intelligent adsorption layer; the TPU electrostatic layer is calculated by weight of the following raw materials: 30-60 parts of thermoplastic polyurethane resin, 10-38 parts of polyol, 5-12 parts of diisocyanate, 5-10 parts of chain extender and 3-10 parts of static eliminator; The preparation method of the TPU thermoplastic polyurethane electrostatic layer comprises the following steps: the first step is to prepare the raw materials with quantitative proportion; Step 2: Put polyol and diisocyanate into a reaction container, and control the temperature to be in the range of 48-100°C and the reaction time T to be 0.5-2.5h to obtain prepolymer a; The third step is to add thermoplastic polyurethane resin, chain extender and static eliminator to the obtained prepolymer a, and control the temperature value range to be 110-150°C and the reaction time T to be 1.5-2h; the generated polymer TPU is mixed, granulated and flattened to form a TPU static layer.
2. A high-toughness car color-changing film as claimed in claim 1, characterized in that: The TPU electrostatic layer is calculated according to the weight parts of the following raw materials: 52 parts of thermoplastic polyurethane resin, 26 parts of polyol, 8 parts of diisocyanate, 10 parts of chain extender and 4 parts of static eliminator.
3. The high-toughness car color-changing film according to claim 1, characterized in that: The TPU electrostatic layer is calculated according to the weight parts of the following raw materials: 48 parts of thermoplastic polyurethane resin, 27 parts of polyol, 12 parts of diisocyanate, 7 parts of chain extender and 6 parts of static eliminator.
4. The high-toughness car color-changing film according to claim 1, characterized in that: The hardness of the thermoplastic polyurethane resin is 35A-80A.
5. A high-toughness car color-changing film as described in any one of claims 1 to 4, characterized in that: The static eliminator includes one of a higher alcohol sulfate ester salt, an aliphatic sulfonate salt, or a higher alcohol phosphate ester salt.
6. A method for preparing a high-toughness automobile color-changing film as claimed in any one of claims 1 to 5, characterized in that: The following steps are included S1, heating the TPH material repair coating, the rebound toughness layer, the TPU electrostatic layer and the nano smart adsorption layer at 120° C. to fuse and stack the TPH material repair coating, the rebound toughness layer, the TPU electrostatic layer and the nano smart adsorption layer together to obtain a fused stacking layer A; S2, compounding the carbon crystal wear-resistant layer on the surface of the fused stacking layer A obtained in step S1 to obtain a composite film B; S3. The composite film B obtained in step S2 is allowed to stand at a temperature of 82-95°C for 72-96 hours, then placed in a cooling machine for cooling, and wound up using a winding device to obtain a high-strength and tough automobile color-changing film.
7. The preparation method according to claim 6, characterized in that: In step S3 , the standing temperature is 90° C., and the standing time T is 90 h.