Modified phosphoric acid ferric pyrophosphate, modified phosphoric acid ferric sodium pyrophosphate and preparation method of modified phosphoric acid ferric pyrophosphate and modified phosphoric acid ferric sodium pyrophosphate

By regulating the stabilization effect of iron source, phosphorus source ratio and carbon-containing complexing agent, combined with sintering reaction, modified iron pyrophosphate and modified sodium phosphate sodium pyrophosphate are prepared, and the existing materials have been solved. The problem of poor stability has achieved a high-performance sodium ion battery positive electrode material.

CN118929593APending Publication Date: 2024-11-12BEI JING XI BEI DONG LI KE JI YOU XIAN GONG SI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410984688.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing sodium ferric pyrophosphate positive electrode materials have low capacity and poor batch stability, which cannot meet the requirements of sodium ion batteries for high-performance positive electrode materials.

Method used

By regulating the iron source, phosphorus source ratio and the stabilization effect of carbon-containing complexing agent, combined with one-step sintering and solid-phase sintering reaction, a modified iron pyrophosphate and modified sodium ferric pyrophosphate positive electrode material is prepared to achieve The iron-phosphorus ratio is stable and controllable, and has high capacity and high rate performance.

Benefits of technology

The prepared cathode material has high capacity, high rate performance and cycle stability, simple process and low raw material cost, and is suitable for sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929593A_ABST
    Figure CN118929593A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of positive electrode materials, in particular to modified ferric pyrophosphate, modified ferric sodium pyrophosphate and a preparation method thereof. Modified ferric pyrophosphate is prepared by regulating the ratio of an iron source to a phosphorus source and the stabilization effect of a carbon-containing complexing agent and combining with one-step sintering, and then the modified ferric sodium pyrophosphate positive electrode material is prepared by utilizing a solid-phase sintering reaction on the basis. The preparation method is simple in process, stable and controllable preparation of the modified ferric sodium pyrophosphate positive electrode material can be achieved through two-step sintering, the raw material cost is low, and the prepared positive electrode material has excellent electrochemical performance such as high capacity, high rate performance and cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of positive electrode materials, and in particular to a modified phosphate iron pyrophosphate, a modified phosphate sodium iron pyrophosphate and a preparation method thereof, and specifically to a modified phosphate iron pyrophosphate, a modified phosphate sodium iron pyrophosphate and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art

[0002] In modern society, batteries have become an indispensable source of energy supply for various electronic devices. Among them, lithium-ion batteries and sodium-ion batteries have attracted much attention and are widely used in various energy storage scenarios. Compared with lithium-ion batteries, sodium-ion batteries have the advantages of high earth abundance of raw materials, low price, stable low-temperature performance, excellent rate performance, and good safety. They will definitely occupy an important position in energy storage, two-wheeled vehicles, high-power and low-temperature application scenarios.

[0003] Positive electrode materials account for the highest proportion of cost and mass in batteries. Polyanionic phosphate electrode materials, especially iron-based sodium iron pyrophosphate, have become a hot research topic for positive electrode materials of sodium ion batteries due to their low cost, high stability and safety. However, existing sodium iron pyrophosphate mainly uses iron phosphate, sodium dihydrogen phosphate, ammonium dihydrogen phosphate and sodium pyrophosphate as phosphorus sources, and directly obtains sodium iron pyrophosphate through one-step sintering. The sodium iron pyrophosphate obtained by this method has low capacity and poor batch stability, which cannot meet the requirements of sodium ion batteries for high-performance positive electrode materials.

[0004] Therefore, it is of great significance to provide a new preparation method of sodium iron phosphate pyrophosphate positive electrode material to improve its performance. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a modified phosphate iron pyrophosphate, a modified phosphate sodium iron pyrophosphate and a preparation method thereof, specifically a modified phosphate iron pyrophosphate, a modified phosphate sodium iron pyrophosphate and a preparation method thereof, a positive electrode sheet and a sodium ion battery. The present invention prepares the modified phosphate iron pyrophosphate by regulating the ratio of the iron source and the phosphorus source and the stabilizing effect of the carbon-containing complexing agent and combining one-step sintering, and then prepares the modified phosphate sodium iron pyrophosphate positive electrode material by solid phase sintering reaction on this basis. The preparation method has a simple process, and the modified phosphate sodium iron pyrophosphate positive electrode material can be prepared stably and controllably by two-step sintering, and the raw material cost is low. The prepared positive electrode material has excellent electrochemical properties such as high capacity, high rate performance and cycle stability.

[0006] In a first aspect, the present invention provides a method for preparing modified phosphoric acid ferric pyrophosphate, the preparation method comprising: mixing an iron source, a phosphorus source, a solvent water, an oxidant and a carbon-containing complexing agent for reaction, followed by drying and sintering to obtain the modified phosphoric acid ferric pyrophosphate.

[0007] The present invention utilizes the stabilizing effect of an iron source, a phosphorus source and a carbon-containing complexing agent and combines it with a one-step sintering to prepare carbon-doped phosphate iron pyrophosphate, namely the modified phosphate iron pyrophosphate of the present invention, so that the iron-phosphorus ratio of the modified phosphate iron pyrophosphate is stable and controllable, and the preparation method is simple and has low raw material cost.

[0008] As a preferred technical solution of the present invention, the oxidant is selected from any one or more of hydrogen peroxide (H2O2), potassium permanganate or oxygen, preferably hydrogen peroxide. When hydrogen peroxide is used as an oxidant, other polluting elements will not be introduced and the operation is simpler.

[0009] As a preferred technical solution of the present invention, the carbon-containing complexing agent is selected from any one or more of ethylenediaminetetraacetic acid, citric acid, aminotriacetic acid or diethylenetriaminepentaacetic acid.

[0010] The carbon-containing complexing agent provided by the invention not only plays a role in stabilizing the ratio of the iron source and the phosphorus source, but also can provide conductive carbon to prepare carbon-doped phosphoric acid iron pyrophosphate.

[0011] As a preferred technical solution of the present invention, the iron source is selected from any one or more of iron powder (Fe), ferrosoferric oxide (Fe3O4), ferrous oxide (Fe2O3) or ferrous oxide (FeO).

[0012] As a preferred technical solution of the present invention, the phosphorus source is selected from any one or more of phosphoric acid (H3PO4), diammonium phosphate (NH4H2PO4) or diammonium hydrogen phosphate ((NH4)2HPO4).

[0013] In the preparation method provided by the present invention, the above-mentioned raw materials are all common raw materials with low cost.

[0014] As a preferred technical solution of the present invention, the molar ratio of the iron element in the iron source to the phosphorus element in the phosphorus source is 0.5-0.9:1, for example, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, etc.

[0015] The invention realizes controllable iron-phosphorus ratio of modified phosphate iron pyrophosphate and final product modified sodium phosphate iron pyrophosphate by regulating the molar ratio of the iron source and the phosphorus source.

[0016] As a preferred technical solution of the present invention, the molar ratio of the oxidant to the iron element in the iron source is 0.5-2:1, for example, 0.5:1, 0.8:1, 1:1, 1.5:1, 2:1, etc.

[0017] As a preferred technical solution of the present invention, the molar ratio of the carbon-containing complexing agent to the iron element in the iron source is 0.8-3:1, for example, 0.8:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, etc., preferably 1-2.5:1.

[0018] When the molar ratio of each raw material is within the scope of the present invention, the obtained modified phosphoric acid ferric pyrophosphate and the final product modified phosphoric acid sodium ferric pyrophosphate have more excellent rate performance and cycle performance.

[0019] As a preferred technical solution of the present invention, the reaction temperature is 90-150°C, and the reaction time is 2-5h. The 90-150°C can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., and the 2-5h can be 2h, 3h, 4h, 5h, etc.

[0020] As a preferred technical solution of the present invention, the drying is spray drying, and the air inlet temperature is 200-280°C, for example, 200°C, 220°C, 240°C, 260°C, 280°C, etc.; the air outlet temperature is 80-120°C, for example, 80°C, 90°C, 100°C, 110°C, 120°C, etc.

[0021] As a preferred technical solution of the present invention, the sintering is sintering at 500-800℃ in an inert gas atmosphere for 3-12h, and the 500-800℃ can be 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, 800℃, etc.; the 3-12h can be 3h, 5h, 7h, 9h, 11h, 12h, etc.; the inert gas can be nitrogen or argon, etc.

[0022] As a specific embodiment of the present invention, the preparation method includes: mixing the iron source, phosphorus source and solvent water evenly, adding an oxidant and mixing evenly, adding a carbon-containing complexing agent and mixing evenly, reacting, and then drying and sintering to obtain the modified phosphoric acid ferric pyrophosphate.

[0023] In the present invention, after adding the oxidant into the reaction system, the mixture is fully stirred for 3-10 hours to be evenly mixed, and then the carbon-containing complexing agent is added to react, so that the reaction is more stable and controllable.

[0024] In a second aspect, the present invention provides modified phosphoric acid ferric pyrophosphate prepared by the preparation method described in the first aspect.

[0025] The modified phosphate iron pyrophosphate prepared by the present invention can achieve a stable and controllable iron-phosphorus ratio, and on this basis, the iron-phosphorus ratio of the modified sodium phosphate iron pyrophosphate can be stably controlled, thereby having excellent electrochemical properties and improving its comprehensive performance and application potential.

[0026] In a third aspect, the present invention provides a method for preparing modified sodium ferric phosphate pyrophosphate, the preparation method comprising: mixing the modified sodium ferric phosphate pyrophosphate described in the second aspect with a sodium source and a carbon source, and calcining to obtain the modified sodium ferric phosphate pyrophosphate.

[0027] The modified sodium ferric phosphate pyrophosphate obtained by the preparation method of the present invention has a core-shell structure, wherein the core is carbon-doped sodium ferric phosphate pyrophosphate and the shell is a carbon coating layer.

[0028] The present invention uses a solid phase sintering reaction to prepare a modified sodium ferric phosphate pyrophosphate positive electrode material based on the prepared modified phosphate ferric pyrophosphate, which has high capacity, excellent rate performance and cycle performance. The preparation method of the present invention has low raw material cost and simple process. The modified sodium ferric phosphate pyrophosphate positive electrode material can be stably and controllably prepared by sintering in two steps. The obtained positive electrode material has excellent electrochemical properties. Specifically:

[0029] The present invention prepares modified phosphate iron pyrophosphate by regulating the ratio of iron source and phosphorus source and the stabilizing effect of carbon-containing complexing agent and combining one-step sintering, wherein the carbon-containing complexing agent provides conductive carbon while playing the role of stabilizing the ratio of iron source and phosphorus source, forming carbon-doped modified phosphate iron pyrophosphate, on which solid phase sintering is performed to form a modified phosphate sodium iron pyrophosphate positive electrode material with a uniform carbon coating layer, and the front and rear two-step sintering uses different carbon sources to effectively improve the electronic conductivity of the modified phosphate sodium iron pyrophosphate positive electrode material, and can inhibit the side reaction between the electrode active material and the electrolyte, ensure the rapid transmission of sodium ions, effectively improve the rate performance of the modified phosphate sodium iron pyrophosphate positive electrode material, and have broad application prospects. And the preparation method of the present invention has low raw material cost and simple process, and realizes the stable and controllable preparation of modified phosphate sodium iron pyrophosphate positive electrode materials with different iron-phosphorus ratios.

[0030] The time for mixing the modified phosphate ferric pyrophosphate with the sodium source and the carbon source is adjusted according to the actual situation, generally 2-10 hours.

[0031] As a preferred technical solution of the present invention, the molar ratio of the modified phosphoric acid ferric pyrophosphate to the sodium element in the sodium source is 1:(4-6), such as 1:4, 1:5, 1:6, etc.

[0032] As a preferred technical solution of the present invention, the content of the carbon element in the carbon source in the modified sodium ferric phosphate pyrophosphate is 1-5wt%, such as 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, etc. The carbon source of the present invention forms a carbon coating layer of the modified sodium ferric phosphate pyrophosphate, that is, the carbon coating amount of the modified sodium ferric phosphate pyrophosphate is 1-5wt%.

[0033] As a preferred technical solution of the present invention, the sodium source is selected from any one or more of sodium carbonate (Na2CO3), sodium nitrate (NaNO3), sodium acetate (CH3COONa) or sodium bicarbonate (NaHCO3).

[0034] As a preferred technical solution of the present invention, the carbon source is selected from any one or more of glucose, sucrose, carbon nanotubes, carbon black or graphene.

[0035] The above raw materials in the preparation method provided by the present invention are all common raw materials with low cost.

[0036] As a preferred technical solution of the present invention, the calcination is calcined at 500-650°C in an inert gas atmosphere for 8-20h, and the 500-650°C can be 500°C, 550°C, 600°C, 650°C, etc.; the 8-20h can be 8h, 10h, 12h, 14h, 16h, 18h, 20h, etc.; the inert gas can be nitrogen or argon.

[0037] In a fourth aspect, the present invention provides modified sodium iron pyrophosphate prepared by the preparation method described in the third aspect.

[0038] The modified sodium iron phosphate pyrophosphate prepared by the invention has excellent electrochemical properties such as high capacity, good cycle performance and rate performance.

[0039] In a fifth aspect, the present invention provides a positive electrode plate, wherein the positive electrode plate comprises the modified sodium iron phosphate pyrophosphate described in the fourth aspect.

[0040] In a sixth aspect, the present invention provides a sodium ion battery, comprising the positive electrode sheet described in the fifth aspect.

[0041] The technical solution provided by the embodiment of the present invention has the following advantages compared with the prior art:

[0042] 1. The present invention prepares modified phosphate iron pyrophosphate by regulating the ratio of iron source and phosphorus source and the stabilizing effect of carbon-containing complexing agent and combining one-step sintering, and then prepares modified phosphate iron sodium pyrophosphate positive electrode material by solid phase sintering reaction. The preparation method is simple, and the modified phosphate iron sodium pyrophosphate positive electrode material can be stably and controllably prepared by two-step sintering, and the raw material cost is low.

[0043] 2. The positive electrode material prepared by the present invention has excellent electrochemical properties such as high capacity, high rate performance and cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0046] Figure 1 This is a lattice structure diagram of the modified phosphoric acid ferric pyrophosphate prepared in Example 1 of the present invention;

[0047] Figure 2 This is the XRD pattern of the modified sodium iron pyrophosphate prepared in Example 1 of the present invention;

[0048] Figure 3 The first charge-discharge curve of the half-cell assembled with the modified sodium iron phosphate pyrophosphate prepared in Example 1 of the present invention at a cycle rate of 0.1C;

[0049] Figure 4 This is a cycle performance diagram of a half-cell assembled with modified sodium iron phosphate pyrophosphate prepared in Example 1 of the present invention at a rate of 1C;

[0050] Figure 5 This is a rate performance diagram of a half-cell assembled with modified sodium iron phosphate pyrophosphate prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0051] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0052] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0053] Example 1

[0054] This embodiment provides a modified phosphate ferric pyrophosphate, a modified sodium ferric pyrophosphate and a preparation method thereof, wherein the preparation method comprises the following steps:

[0055] (1) 3 mol of iron powder (Fe) and 4 mol of phosphoric acid (H3PO4) were mixed, 5 mol of hydrogen peroxide (H2O2) was added, and the mixture was stirred for 5 h. 3 mol of ethylenediaminetetraacetic acid was added and the mixture was transferred to a reactor to continue the reaction for 4 h. The temperature of the reactor was 110° C.; spray drying was then performed. The inlet air temperature of the spray drying was 240° C. and the outlet air temperature was 100° C. The spray-dried material was sintered in a tubular furnace at 650° C. under nitrogen protection for 6 h to obtain the modified phosphate iron pyrophosphate (carbon-doped phosphate iron pyrophosphate). The lattice structure of the modified phosphate iron pyrophosphate is shown in the figure below. Figure 1 As shown;

[0056] (2) 1 mol of modified phosphate iron pyrophosphate, 2 mol of sodium carbonate (Na2CO3) and carbon nanotubes are fully mixed for 5 h, wherein the mass of the carbon source is calculated based on the carbon coating amount of the final product modified phosphate iron sodium pyrophosphate being 2 wt%, and then the above powder is sintered at 600 ° C for 10 h in a tube furnace under nitrogen or argon protective gas, and after cooling to room temperature, the modified phosphate iron sodium pyrophosphate positive electrode material is obtained, and its XRD pattern is as shown Figure 2 shown.

[0057] Example 2

[0058] This embodiment provides a modified phosphate ferric pyrophosphate, a modified sodium ferric pyrophosphate and a preparation method thereof, wherein the preparation method comprises the following steps:

[0059] (1) 0.8 mol of ferrosoferric oxide (Fe3O4) and 4 mol of phosphoric acid (H3PO4) were mixed, 1.26 mol of hydrogen peroxide (H2O2) was added, and the mixture was stirred for 7 hours. Then, 3.2 mol of ethylenediaminetetraacetic acid was added and the mixture was transferred to a reactor and the reaction was continued for 3 hours. The temperature of the reactor was 125°C. Then, spray drying was performed. The inlet air temperature of the spray drying was 260°C and the outlet air temperature was 95°C. The spray-dried material was sintered in a tubular furnace at 750°C under nitrogen protection for 4 hours to obtain the modified phosphoric acid pyrophosphate iron (carbon-doped phosphoric acid pyrophosphate iron);

[0060] (2) 1 mol of modified ferric phosphate pyrophosphate, 4 mol of sodium bicarbonate (NaHCO3) and glucose (C6H 12 O6) is fully mixed for 3 hours, wherein the mass of the carbon source is calculated based on the carbon coating amount of the final product modified sodium iron phosphate pyrophosphate as 3wt%, and then the above powder is sintered at 550°C for 15 hours in a tubular furnace under nitrogen or argon protective gas, and then cooled to room temperature to obtain the modified sodium iron phosphate pyrophosphate positive electrode material.

[0061] Example 3

[0062] This embodiment provides a modified phosphate ferric pyrophosphate, a modified sodium ferric pyrophosphate and a preparation method thereof, wherein the preparation method comprises the following steps:

[0063] (1) 2.2 mol of iron powder (Fe) and 4 mol of ammonium dihydrogen phosphate (NH4H2PO4) were mixed, 3.6 mol of hydrogen peroxide (H2O2) was added, and the mixture was stirred for 8 h. After 5.5 mol of ethylenediaminetetraacetic acid was added, the mixture was transferred to a reactor and continued to react for 3 h. The temperature of the reactor was 140°C. Spray drying was then performed. The inlet air temperature of the spray drying was 220°C and the outlet air temperature was 85°C. The spray-dried material was sintered in a tubular furnace at 550°C under nitrogen protection for 10 h to obtain the modified phosphoric acid pyrophosphate iron (carbon-doped phosphoric acid pyrophosphate iron);

[0064] (2) 1 mol of modified ferric phosphate pyrophosphate, 4 mol of sodium nitrate (NaNO3) and sucrose (C 12 H 22 O 11 ) are fully mixed for 7 hours, wherein the mass of the carbon source is calculated based on the carbon coating amount of the final product modified sodium iron phosphate pyrophosphate being 3wt%, and then the above powder is sintered at 525°C for 18 hours in a tubular furnace under nitrogen or argon protective gas, and then cooled to room temperature to obtain the modified sodium iron phosphate pyrophosphate positive electrode material.

[0065] Example 4

[0066] This embodiment provides a modified phosphate ferric pyrophosphate, a modified sodium ferric pyrophosphate and a preparation method thereof, wherein the preparation method comprises the following steps:

[0067] (1) After mixing 1.7 mol of ferric oxide (Fe2O3) and 4 mol of diammonium hydrogen phosphate ((NH4)2HPO4), 4.2 mol of hydrogen peroxide (H2O2) was added and stirred for 4 hours; after adding 3.4 mol of ethylenediaminetetraacetic acid complexing agent, the mixture was transferred to a reactor and fully reacted for 3.5 hours at a temperature of 100°C; spray drying was then performed, and the inlet air temperature of the spray drying was 270°C and the outlet air temperature was 105°C. The spray-dried material was sintered in a tubular furnace at 600°C under nitrogen protection for 8 hours to obtain the modified phosphate iron pyrophosphate (carbon-doped phosphate iron pyrophosphate);

[0068] (2) 1 mol of modified phosphate ferric pyrophosphate, 4 mol of sodium acetate (CH3COONa) and carbon black are fully mixed for 9 hours, wherein the mass of the carbon source is calculated based on the carbon coating amount of the final product modified sodium ferric pyrophosphate as 3wt%, and then the above powder is sintered at 575°C for 14 hours in a tubular furnace under nitrogen or argon protective gas, and then cooled to room temperature to obtain the modified sodium ferric pyrophosphate positive electrode material.

[0069] Example 5

[0070] This embodiment provides a modified phosphate ferric pyrophosphate, a modified sodium ferric pyrophosphate and a preparation method thereof, wherein the preparation method comprises the following steps:

[0071] (1) 2.8 mol of ferrous oxide (FeO) and 4 mol of ammonium dihydrogen phosphate (NH4H2PO4) were mixed, 1.8 mol of hydrogen peroxide (H2O2) was added, and the mixture was stirred for 9 hours. After that, 3 mol of ethylenediaminetetraacetic acid was added and the mixture was transferred to a reactor and continued to react for 4.5 hours. The temperature of the reactor was 95°C. Then, spray drying was performed. The inlet air temperature of the spray drying was 210°C and the outlet air temperature was 85°C. The spray-dried material was sintered in a tubular furnace at 700°C under nitrogen protection for 5 hours to obtain the modified phosphate iron pyrophosphate (carbon-doped phosphate iron pyrophosphate);

[0072] (2) 1 mol of modified phosphate ferric pyrophosphate, 2 mol of sodium carbonate (Na2CO3) and graphene are fully mixed for 6 hours, wherein the mass of the carbon source is calculated based on the carbon coating amount of the final product modified sodium ferric pyrophosphate being 4 wt%. The above powder is then sintered at 550°C for 12 hours in a tubular furnace under nitrogen or argon protective gas, and then cooled to room temperature to obtain the modified sodium ferric pyrophosphate positive electrode material.

[0073] Example 6

[0074] This embodiment provides a modified phosphoric acid ferric pyrophosphate, a modified phosphoric acid sodium ferric pyrophosphate and a preparation method thereof. The preparation method is the same as that of Example 1, except that in this embodiment, the iron powder is 3 mol and the phosphoric acid is 9 mol.

[0075] Example 7

[0076] This embodiment provides a modified phosphate iron pyrophosphate, modified sodium phosphate iron pyrophosphate and a preparation method thereof. The preparation method is the same as that of Example 1, except that in this embodiment, the iron powder is 3 mol and the phosphoric acid is 2 mol.

[0077] Comparative Example 1

[0078] This comparative example provides a phosphate ferric pyrophosphate, modified sodium phosphate ferric pyrophosphate and a preparation method thereof. The preparation method is the same as that of Example 1, and the difference from Example 1 is that no carbon-containing complexing agent is added in this comparative example, that is, carbon-doped phosphate ferric pyrophosphate cannot be formed.

[0079] Comparative Example 2

[0080] The present comparative example provides sodium ferric pyrophosphate and a preparation method thereof, wherein the preparation method comprises: fully mixing 3 mol of ferric phosphate, 1 mol of sodium dihydrogen phosphate, 3 mol of sodium carbonate and 80 g of glucose, and then spray drying after sand milling for 2 hours, wherein the inlet air temperature of the spray drying is 210° C., and the outlet air temperature is 95° C., and the spray-dried material is sintered at 550° C. in a tubular furnace under nitrogen protection for 12 hours to obtain sodium ferric pyrophosphate.

[0081] Performance Testing

[0082] (1) Assembling the battery: The positive electrode material prepared in the embodiment and the comparative example was used as the positive electrode active material, and the positive electrode sheet prepared by mixing Super P conductive carbon and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 was used as the positive electrode, a metal sodium sheet was used as the counter electrode, 5 Vol% fluoroethylene carbonate was added to a 1M NaClO4 / propylene carbonate solution as the electrolyte, and glass fiber was used as the separator. The button battery was assembled in a high-purity argon atmosphere glove box.

[0083] (2) Test method: The electrochemical performance of button cells was tested in a voltage window of 1.8 to 4.2 V.

[0084] The results are shown in Table 1 and Figure 3-5 As shown, Figure 3 The first charge-discharge curve of the half-cell assembled with the modified sodium iron phosphate pyrophosphate prepared in Example 1 of the present invention at a cycle rate of 0.1C is shown in FIG. Figure 4 This is a cycle performance diagram of a half-cell assembled with modified sodium iron phosphate pyrophosphate prepared in Example 1 of the present invention at a rate of 1C. Figure 5 This is a rate performance diagram of a half-cell assembled with modified sodium iron phosphate pyrophosphate prepared in Example 1 of the present invention.

[0085] Table 1

[0086]

[0087]

[0088] From Table 1 and Figure 3-5 It can be found that the theoretical capacity of the positive electrode active material is calculated as 129 mAh / g, and the battery prepared using the modified sodium iron phosphate pyrophosphate positive electrode material prepared by the present invention has a discharge capacity of more than 90 mAh / g at 0.1C, the battery is cycled 100 times at a rate of 1C, and the capacity retention rate is more than 88%, and the discharge capacity at a rate of 30C is more than 31 mAh / g, which has high capacity and excellent rate performance and cycle performance.

[0089] From the comparison between Examples 1 and 6-7, it can be found that when the iron-phosphorus ratio is too high or too low, performance will be reduced; from the comparison between Example 1 and Comparative Examples 1 and 2, it can be found that the modified sodium iron phosphate pyrophosphate provided by the present invention has significantly improved discharge capacity and cycle performance compared with non-carbon-doped sodium iron phosphate pyrophosphate and ordinary sodium iron phosphate pyrophosphate.

[0090] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0091] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments described herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing modified phosphoric acid ferric pyrophosphate, characterized in that: The preparation method comprises: mixing an iron source, a phosphorus source, solvent water, an oxidant and a carbon-containing complexing agent for reaction, and then drying and sintering to obtain the modified phosphoric acid ferric pyrophosphate.

2. The preparation method according to claim 1, characterized in that: The oxidant is selected from any one or more of hydrogen peroxide, potassium permanganate or oxygen; and / or, the carbon-containing complexing agent is selected from any one or more of ethylenediaminetetraacetic acid, citric acid, aminotriacetic acid or diethylenetriaminepentaacetic acid; And / or, the iron source is selected from any one or more of iron powder, ferroferric oxide, ferrous oxide or ferrous oxide; And / or, the phosphorus source is selected from any one or more of phosphoric acid, ammonium dihydrogen phosphate or diammonium hydrogen phosphate.

3. The preparation method according to claim 1 or 2, characterized in that: The molar ratio of the iron element in the iron source to the phosphorus element in the phosphorus source is 0.5-0.9:1; and / or, the molar ratio of the oxidant to the iron element in the iron source is 0.5-2:1; and / or, the molar ratio of the carbon-containing complexing agent to the iron element in the iron source is 0.8-3:1; And / or, the reaction temperature is 90-150°C and the reaction time is 2-5h; And / or, the drying is spray drying, the air inlet temperature is 200-280°C, and the air outlet temperature is 80-120°C; And / or, the sintering is performed at 500-800° C. in an inert gas atmosphere for 3-12 hours.

4. The modified phosphoric acid ferric pyrophosphate prepared by the preparation method according to any one of claims 1 to 3.

5. A method for preparing modified sodium ferric pyrophosphate, characterized in that: The preparation method comprises: mixing the modified phosphoric acid ferric pyrophosphate described in claim 4 with a sodium source and a carbon source, and calcining to obtain the modified phosphoric acid sodium ferric pyrophosphate.

6. The preparation method according to claim 5, characterized in that: The molar ratio of the modified phosphoric acid ferric pyrophosphate to the sodium element in the sodium source is 1:(4-6); And / or, the content of carbon element in the carbon source in the modified sodium ferric phosphate pyrophosphate is 1-5wt%.

7. The preparation method according to claim 5 or 6, characterized in that: The sodium source is selected from any one or more of sodium carbonate, sodium nitrate, sodium acetate or sodium bicarbonate; And / or, the carbon source is selected from any one or more of glucose, sucrose, carbon nanotubes, carbon black or graphene; And / or, the calcination is performed at 500-650° C. in an inert gas atmosphere for 8-20 h.

8. Modified sodium ferric phosphate pyrophosphate prepared by the preparation method according to any one of claims 5 to 7.

9. A positive electrode sheet, characterized in that: The positive electrode plate includes the modified sodium iron phosphate pyrophosphate as described in claim 8.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Iron phosphate and preparation method thereof

    CN107522187A

  • Preparation method of lithium manganese iron phosphate positive electrode material

    CN116216678A

  • Spherical ferric sodium pyrophosphate positive electrode material and preparation method thereof

    CN116344772A

  • Preparation method of sodium ferric manganese phosphate pyrophosphate positive electrode material with core-shell structure

    CN116924371A

  • Modified ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof

    CN117766710A