Quartz sand purification method

Through high-energy ball milling and multi-stage acid leaching technology, combined with vacuum and oxidative roasting, the problem of difficult removal of impurities inside the quartz sand lattice is solved, and quartz sand purification with high purity and high recovery rate is achieved, breaking through the domestic high-purity quartz sand production bottleneck.

CN118929673APending Publication Date: 2024-11-12CHANGSHA SHARPEN ADVANCED MATERIALS CO LTD

Patent Information

Application Number
CN202411170965.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult for the existing technology to purify high-purity quartz sand products, especially the depth removal of the quartz sand lattice, resulting in the domestic high-purity quartz sand heavily relying on imports.

Method used

Using high-energy ball milling, vacuum calcining, oxidative calcining and multi-stage acid leaching technology, the surface energy and internal defects of quartz sand are increased through high-energy ball milling, vacuum calcining promotes the diffusion of impurities to the surface, and multi-stage acid leaching is achieved by using different acid liquid combinations to achieve depth removal. miscellaneous.

Benefits of technology

It achieves high purity (99.9991% and above) and high recovery rate of quartz sand, low impurity content, simple method and low cost, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a purification method of quartz sand. The method comprises the following steps: sequentially carrying out high-energy ball milling, acid leaching I, vacuum roasting, oxidizing roasting and acid leaching II on a quartz sand raw material. The ultra-high-purity quartz sand product can be obtained, the impurity content of the ultra-high-purity quartz sand product is low, the purity can reach 99.9991% or above, the yield is high, the method is simple, the cost is low, and the ultra-high-purity quartz sand product is suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a quartz sand purification method and belongs to the field of quartz sand purification. Background Art

[0002] High-purity quartz sand (≥99.998%, 4N8) has excellent physical and chemical properties such as high temperature resistance, corrosion resistance, low thermal expansion, high insulation, and high light transmittance, and is widely used in semiconductors, photovoltaics, aerospace, and other fields. However, as a key strategic material, high-purity quartz sand products in the current Chinese market are heavily dependent on imports. The root cause is that domestic quartz ore processing and purification technology has not yet achieved a breakthrough, and there is a generation gap compared with foreign technology.

[0003] The quartz ore processing flow mainly consists of two parts: ore pretreatment and quartz sand purification. Among them, quartz sand purification is a key step in the quartz ore processing flow, mainly including acid leaching, ultrasound, roasting, flotation, microwave, magnetic separation, chlorination and other means. Studies have shown that the combination of acid leaching and roasting is a powerful means to reduce the impurity content of quartz sand. At the same time, the characteristics of simple operation and easy scalability give this technology a broad application prospect. However, this scheme is difficult to obtain high-purity quartz sand products. The main reasons are: first, acid leaching only removes impurities on the surface of quartz sand, and it is difficult to achieve deep impurity removal inside the quartz sand lattice; secondly, air or oxygen roasting mainly removes non-metallic impurities such as phosphorus and sulfur, and has a weak effect on substitutional impurity elements and interstitial impurity elements in the quartz sand lattice. In summary, it is urgent to develop a new purification technology for high-purity quartz sand products to break through the bottleneck of existing technologies. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention aims to provide a method for purifying quartz sand. The quartz sand obtained by the method has high purity, good quality and high yield.

[0005] In order to achieve the above technical purpose, the present invention provides a method for purifying quartz sand, which comprises sequentially subjecting the quartz sand raw material to high-energy ball milling, acid leaching I, vacuum roasting, oxidative roasting and acid leaching II to obtain the quartz sand.

[0006] The present invention firstly performs high-energy ball milling on quartz sand to increase its surface energy, put it in a thermodynamically unstable state, reduce the energy barrier for reacting with acid solution, oxidize the surface metal impurities and exist in the form of oxides on the surface of quartz sand, which is more likely to react with acid; secondly, during the high-energy ball milling process, quartz sand powder undergoes strong plastic deformation, the defect concentration inside the lattice increases, deformation energy is accumulated, and diffusion activity is increased; finally, vacuum roasting greatly promotes the diffusion of impurity elements inside the quartz sand lattice to the surface, forms a concentration gradient, and creates favorable conditions for further acid leaching and impurity removal.

[0007] As a preferred solution, the median diameter of the quartz sand raw material is 100 to 500 μm, more preferably 200 to 500 μm, and most preferably 300 to 500 μm.

[0008] As a preferred scheme, the conditions for the high-energy ball milling are: the atmosphere is a protective atmosphere, the pressure is 1.1 to 1.5 atmospheres, more preferably 1.1 to 1.4 atmospheres, and most preferably 1.2 to 1.4 atmospheres; the ball milling speed is 300 to 500 rpm, the ball-to-material ratio is 8 to 16:1, more preferably 8 to 14:1, and most preferably 8 to 12:1; the ball milling time is 2 to 24 hours, more preferably 6 to 24 hours, and most preferably 10 to 24 hours.

[0009] As a preferred solution, the protective atmosphere is nitrogen.

[0010] As a preferred solution, the conditions of the acid leaching I are: using hydrochloric acid as a leaching agent, the liquid-solid mass ratio is 1-6:1, more preferably 2-6:1, and most preferably 3-6:1; the temperature is 60-90°C, more preferably 70-90°C, and most preferably 80-90°C; the stirring speed is 300-600rpm, and the time is 8-16h. This leaching process is a surface leaching, using low-concentration hydrochloric acid to leach impurities on the surface of quartz sand, and the impurity elements form a concentration gradient from the inside of the quartz sand lattice to the surface, creating a chemical potential gradient for the subsequent diffusion of impurities inside the lattice to the surface.

[0011] As a preferred solution, the concentration of the hydrochloric acid is 1 to 6 mol / L, more preferably 2 to 6 mol / L, and most preferably 3 to 6 mol / L.

[0012] As a preferred solution, after the acid leaching process I is completed, dilute hydrochloric acid and water are used for cleaning in sequence. The cleaning process can prevent the precipitation of ion-state impurities such as iron at a higher pH value. After washing with dilute hydrochloric acid for 6 times, water is used for 6 times. The concentration of dilute hydrochloric acid is 0.5-3 mol / L.

[0013] As a preferred solution, the vacuum calcination conditions are: the vacuum degree is 10 -5 ~10 -2 Pa, the temperature is 1000-1400°C, and the time is 2-12h. The further preferred vacuum roasting temperature is 1200-1400°C, and the most preferred vacuum roasting temperature is 1300-1400°C. The present invention enhances the purification effect of quartz sand by controlling the conditions of the vacuum roasting stage within a suitable range. During the vacuum roasting process, if the temperature or vacuum degree is too low, the impurities in the core of the quartz sand cannot diffuse to the surface, which is not conducive to subsequent acid leaching treatment; if the temperature or vacuum degree is too high, the impurities diffused to the surface will be re-dissolved into the interior of the quartz sand, reducing the purification effect.

[0014] As a preferred solution, the oxidation roasting conditions are: oxygen atmosphere, temperature of 1000-1500°C, pressure of 1.1-1.5 atmospheres, and time of 2-12 hours. A further preferred oxidation roasting temperature is 1200-1500°C, and a most preferred oxidation roasting temperature is 1400-1500°C.

[0015] As a preferred solution, the conditions of acid leaching II are: using a mixed acid solution containing inorganic acid, organic acid, sodium salt and crown ether as a leaching agent, the liquid-solid mass ratio is 1-8:1, the temperature is 70-90°C, and the time is 12-24h. The acid leaching process is based on Lewis acid-base theory, using the characteristics that acids containing lone pairs of electrons and ionic impurities with empty orbitals can form complexes, and combining high-concentration strong acid leaching to achieve efficient purification of quartz sand.

[0016] As a preferred embodiment, the molar ratio of the inorganic acid, organic acid, sodium salt and crown ether compound is (12-20):(0.04-0.14):(0.01-0.06):(0.002-0.008).

[0017] As a preferred solution, the inorganic acid includes hydrochloric acid and nitric acid.

[0018] As a preferred solution, the molar ratio of hydrochloric acid to nitric acid is 4-8:8-12.

[0019] As a preferred solution, the concentration of the hydrochloric acid in the mixed acid solution is 4-8 mol / L.

[0020] As a preferred solution, the concentration of nitric acid in the mixed acid solution is 8-12 mol / L.

[0021] As a preferred solution, the organic acid includes oxalic acid and citric acid. Oxalic acid and citric acid can complex transition metal elements.

[0022] As a preferred solution, the molar ratio of oxalic acid to citric acid is 0.02-0.08:0.02-0.06.

[0023] As a preferred solution, the concentration of oxalic acid in the mixed acid solution is 0.02-0.08 mol / L.

[0024] As a preferred solution, the concentration of citric acid in the mixed acid solution is 0.02-0.06 mol / L.

[0025] As a preferred solution, the sodium salt is disodium ethylenediaminetetraacetate. Sodium salt is mainly used to chelate metals such as potassium, calcium, and manganese, which can enhance the purification effect.

[0026] As a preferred solution, the concentration of the sodium salt in the mixed acid solution is 0.01-0.06 mol / L.

[0027] As a preferred solution, the crown ether compounds include 15-crown ether-5, 18-crown ether-6 and 12-crown ether-4. The crown ether compounds are mainly used for complexing sodium ions to achieve deep purification of quartz sand.

[0028] As a preferred embodiment, the molar ratio of 15-crown-5, 18-crown-6 and 12-crown-4 is (0.5-1):(1-2):(0.5-1).

[0029] As a preferred solution, the concentration of the crown ether compound in the mixed acid solution is 0.002-0.008 mol / L.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The purified quartz sand product has high purity (can reach 99.9991% and above), low impurity content, good quality, and high yield (recovery rate is nearly 100%);

[0032] (2) The substitutional and interstitial impurities existing in the quartz sand are diffused to the surface by vacuum diffusion, and the quartz sand is deeply removed by acid leaching. The method is simple, low-cost and suitable for industrial application. DETAILED DESCRIPTION

[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] (1) Quartz sand powder with a median diameter of 300 μm was selected for ball milling. The ball milling conditions were: nitrogen pressure of 1.2 atmospheres, ball milling speed of 500 rpm, ball-to-material ratio of 8:1, and ball milling time of 24 h.

[0036] (2) The ball-milled quartz sand was placed in a polytetrafluoroethylene beaker, and 3 mol / L hydrochloric acid was added, with a liquid-to-solid mass ratio of 3:1, a water bath temperature of 80°C, a stirring speed of 500 rpm, and a leaching time of 12 h. After the leaching was completed, the quartz sand was washed 6 times with 0.5 mol / L dilute hydrochloric acid, and then washed 6 times with deionized water, and the quartz sand was dried for later use.

[0037] (3) The quartz sand treated in the previous step is placed in a quartz crucible for vacuum calcination at a temperature of 1300°C and a vacuum degree of 10 -3 Pa, the time is 12 hours.

[0038] (4) The quartz sand treated in the previous step is placed in a quartz crucible and calcined for 12 hours in an oxygen atmosphere at a pressure of 1.2 atmospheres and a temperature of 1400°C.

[0039] (5) Transfer the quartz sand treated in the previous step to a polytetrafluoroethylene beaker, add a chemical reagent with a certain composition ratio as a leaching agent, and perform mixed acid leaching by water bath heating. The main components of the chemical reagent include hydrochloric acid (the concentration in the leaching agent is 6 mol / L), nitric acid (the concentration in the leaching agent is 8 mol / L), oxalic acid (the concentration in the leaching agent is 0.03 mol / L), citric acid (the concentration in the leaching agent is 0.06 mol / L), disodium ethylenediaminetetraacetate (the concentration in the leaching agent is 0.02 mol / L), and crown ether compounds (the concentration in the leaching agent is 0.008 mol / L, including 15-crown-5, 18-crown-6 and 12-crown-4, and the corresponding molar ratio is 1:2:1); the liquid-solid mass ratio is 8:1, the water bath temperature is 90°C, the time is 12 hours, and the stirring speed is 500 rpm.

[0040] The purity of the quartz sand product obtained by purification under the conditions of this embodiment is 99.9991%.

[0041] Example 2

[0042] (1) Quartz sand powder with a median diameter of 300 μm was selected for ball milling. The ball milling conditions were: nitrogen pressure of 1.2 atmospheres, ball milling speed of 500 rpm, ball-to-material ratio of 8:1, and ball milling time of 24 h.

[0043] (2) The ball-milled quartz sand was placed in a polytetrafluoroethylene beaker, and 3 mol / L hydrochloric acid was added, with a liquid-to-solid mass ratio of 3:1, a water bath temperature of 80°C, a stirring speed of 500 rpm, and a leaching time of 12 h. After the leaching was completed, the quartz sand was washed 6 times with 0.5 mol / L dilute hydrochloric acid, and then washed 6 times with deionized water, and the quartz sand was dried for later use.

[0044] (3) The quartz sand treated in the previous step is placed in a quartz crucible for vacuum calcination at a temperature of 1400°C and a vacuum degree of 10 -5 Pa, the time is 12 hours.

[0045] (4) The quartz sand treated in the previous step is placed in a quartz crucible and calcined for 12 hours in an oxygen atmosphere at a pressure of 1.2 atmospheres and a temperature of 1400°C.

[0046] (5) Transfer the quartz sand treated in the previous step to a polytetrafluoroethylene beaker, add a chemical reagent with a certain composition ratio as a leaching agent, and perform mixed acid leaching by water bath heating. The main components of the chemical reagent include hydrochloric acid (the concentration in the leaching agent is 6 mol / L), nitric acid (the concentration in the leaching agent is 8 mol / L), oxalic acid (the concentration in the leaching agent is 0.03 mol / L), citric acid (the concentration in the leaching agent is 0.06 mol / L), disodium ethylenediaminetetraacetate (the concentration in the leaching agent is 0.02 mol / L), and crown ether compounds (the concentration in the leaching agent is 0.008 mol / L, including 15-crown-5, 18-crown-6 and 12-crown-4, and the corresponding molar ratio is 1:2:1); the liquid-solid mass ratio is 8:1, the water bath temperature is 90°C, the time is 12 hours, and the stirring speed is 500 rpm.

[0047] The purity of the quartz sand product obtained by purification under the conditions of this embodiment is 99.9992%.

[0048] Comparative Example 1

[0049] The quartz sand raw material is purified by the method of Example 1, except that the temperature of the vacuum calcination in step (3) is controlled to be 900°C.

[0050] The purity of the quartz sand product obtained under the conditions of this comparative example is 99.997%.

[0051] Comparative Example 2

[0052] The quartz sand raw material was purified by the method of Example 1, except that the vacuum degree of the vacuum roasting in step (3) was controlled to be 10 -1 Pa.

[0053] The purity of the quartz sand product obtained under the conditions of this comparative example is 99.996%.

[0054] Comparative Example 3

[0055] The quartz sand raw material was purified by the method of Example 1, except that the vacuum degree of the vacuum roasting in step (3) was controlled to be 10 -6 Pa.

[0056] The purity of the quartz sand product obtained under the conditions of this comparative example is 99.993%.

[0057] Comparative Example 4

[0058] The quartz sand raw material is purified by the method of Example 1, except that the temperature of the vacuum calcination in step (3) is controlled to be 1450°C.

[0059] The purity of the quartz sand product obtained under the conditions of this comparative example is 99.995%.

[0060] Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for purifying quartz sand, Features: The quartz sand raw material is subjected to high-energy ball milling, acid leaching I, vacuum roasting, oxidation roasting and acid leaching II in sequence to obtain the quartz sand.

2. A method for purifying quartz sand according to claim 1, Features: The median diameter of the quartz sand raw material is 100-500 μm.

3. A method for purifying quartz sand according to claim 1 or 2, Features: The conditions of the high-energy ball milling are as follows: the atmosphere is a protective atmosphere, the pressure is 1.1 to 1.5 atmospheres, the ball milling speed is 300 to 500 rpm, the ball-to-material ratio is 8 to 16:1, and the ball milling time is 2 to 24 hours.

4. A method for purifying quartz sand according to claim 1, Features: The conditions of the acid leaching I are: using hydrochloric acid as the leaching agent, the liquid-to-solid mass ratio is 1-6:1, the temperature is 60-90°C, and the time is 8-16h.

5. A method for purifying quartz sand according to claim 4, Features: The concentration of the hydrochloric acid is 1-6 mol / L.

6. A method for purifying quartz sand according to claim 1, Features: The vacuum calcination conditions are: vacuum degree of 10 -5 ~10 -2 Pa, temperature is 1000~1400℃, time is 2~12h.

7. A method for purifying quartz sand according to claim 6, Features: The temperature of vacuum calcination is 1300-1400°C.

8. A method for purifying quartz sand according to claim 1, Features: The conditions for the oxidation roasting are: an oxygen atmosphere, a temperature of 1000-1500° C., a pressure of 1.1-1.5 atmospheres, and a time of 2-12 hours.

9. A method for purifying quartz sand according to claim 1, Features: The conditions of the acid leaching II are: using a mixed acid solution containing inorganic acid, organic acid, sodium salt and crown ether compound as a leaching agent, the liquid-to-solid mass ratio is 1 to 8:1, the temperature is 70 to 90°C, and the time is 12 to 24 hours.

10. A method for purifying quartz sand according to claim 9, Features: The molar ratio of the inorganic acid, organic acid, sodium salt and crown ether compound is (12-20):(0.04-0.14):(0.01-0.06):(0.002-0.008); The inorganic acid includes hydrochloric acid and nitric acid; The organic acid includes oxalic acid and citric acid; The sodium salt is disodium ethylenediaminetetraacetate; The crown ether compounds include 15-crown-5, 18-crown-6 and 12-crown-4.

Citation Information

Patent Citations

  • Purification method for high-purity quartz with ultra-low metal elements

    CN102674372A

  • Method for refining high-purity quartz sand from ordinary quartz sand

    CN107555442A

  • A method for preparing high-purity quartz sand powder used for electronic products by utilizing quartzite containing feldspar

    CN109534347A

  • Method for purifying quartz sands by microwave-vacuum combined roasting

    CN112010317A

Cited By

  • Alaite type high-purity quartz sand and directional impurity removal method thereof

    CN120172419A