Method for preparing transition metal disulfide monolayer by aqueous-phase large-scale stripping

Two-dimensional transition metal dichalcogenide monolayers were prepared by using a probe-based ultrasonic cavitation mechanical exfoliation method in water, which solved the problems of material decomposition and contamination in the preparation process of existing technologies, and enabled the application of high-concentration and high-stability two-dimensional materials.

CN118929764AActive Publication Date: 2024-11-12OCEAN UNIV OF CHINA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411131403.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-18
Publication Date
2024-11-12
Estimated Expiration
2044-08-18

AI Technical Summary

Technical Problem

Existing technologies make it difficult to efficiently and on a large scale prepare high-concentration two-dimensional transition metal dichalcogenide monolayers in water, and the use of organic solvents in the preparation process can lead to material decomposition and pollution, which limits their application in electronic products.

Method used

A probe-based ultrasonic cavitation mechanical exfoliation method was used to prepare two-dimensional transition metal dichalcogenide monolayers in water through lithium pre-intercalation and ultrasonic treatment, avoiding the use of chemical additives and achieving large-scale layering.

Benefits of technology

The prepared two-dimensional transition metal dichalcogenide monolayer exhibits high concentration and high stability in water, and can be mixed with other materials to form multifunctional composite materials suitable for the manufacture of electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004997986630000011
    Figure HDA0004997986630000011
  • Figure HDA0004997986630000012
    Figure HDA0004997986630000012
  • Figure HDA0004997986630000013
    Figure HDA0004997986630000013
Patent Text Reader

Abstract

The invention discloses a method for preparing a transition metal disulfide monolayer through water-phase large-scale stripping, and belongs to the technical field of new material preparation. According to the invention, large-scale layering can be carried out on wide-range TMDs in water under the condition that no chemical additive is used in the liquid stripping process; the pre-intercalated TMD phase is layered in water using probe ultrasonic cavitation mechanical exfoliation to produce various TMD monolayers. Water is used as a solvent, the cost is low, no additive is used, and the problem that the added additive is attached to the surface of the TMD sheet to affect the overall performance of the TMD sheet is solved. The prepared TMD is high in single-piece yield, can be prepared on a large scale, and is high in concentration and high in stability. The prepared two-dimensional TMD can be mixed and combined with a series of functional materials to form a two-dimensional multifunctional heterostructure, a stable colloidal dispersion can be formed under high concentration, and a multifunctional platform is provided for assembling various multifunctional composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new material preparation, and in particular relates to a method for preparing a transition metal dichalcogenide monolayer by large-scale aqueous phase exfoliation. Background Art

[0002] Two-dimensional (2D) transition metal dichalcogenides (TMDs), as a class of 2D materials other than graphene, have great potential applications in various fields ranging from optics to electronics, optoelectronics, energy storage, and catalysis. Compared with graphene, they have tunable band gaps. For example, molybdenum disulfide (MoS2), one of the main TMDs, has a band gap of up to 1.9 eV for a single monolayer, but its band gap decreases with increasing layer thickness due to quantum confinement. Benefiting from its direct band gap, MoS2 monolayer shows excellent electrical properties, such as high in-plane mobility and high current on / off ratio, which makes it an attractive channel material for low-power and high-performance transistors. High-quality and stable TMD monolayer materials are ideal material candidates for hydrogels, biocomposites, and green electronics.

[0003] So far, the methods for preparing single-layer and multilayer 2D TMD nanosheets include mechanical exfoliation, CVD growth, chemical / electrochemical lithium intercalation and exfoliation, and liquid-phase exfoliation in organic solvents. However, the main problems of organic lithium intercalation and exfoliation methods in organic solvents are low yield of TMD monolayer sheets, low concentration, decomposition into subnanoscale sheets, variable thickness, and formation of metal nanoparticles and Li2S precipitation. These problems limit the development of solution-processed TMDs in applications such as thin-film electronics that require clean and large-sized sheets. In addition, electrochemical intercalation of lithium or organic molecules (such as tetraheptyl ammonium cations or hydrazine) can exfoliate high-quality MoS2 and WS2 monolayers in organic solvents, but these methods require expensive large TMD single crystals as cathodes for the intercalation reaction. In addition, almost most of the above-mentioned TMD flakes must be dispersed in toxic organic solvents such as isopropanol, n-methylpyrrolidone or dimethyl sulfoxide. In existing reports, 2D MXenes in water can be LbL assembled with near-monolayer accuracy each time they are deposited, but 2D TMD monolayers are difficult to use for this LbL process unless they are dispersed in water. In addition, the lack of water-based 2D TMDs also limits their combination with large-scale water-dispersible nanomaterials (such as MXene, graphene, and nanocellulose) into 2D multifunctional heterostructures. The door to the above possibilities is currently closed to 2D TMDs unless they can be exfoliated into highly concentrated monolayer solutions in water. Therefore, the fabrication of highly concentrated 2D TMD monolayers dispersed in water is of great significance for practical applications. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a transition metal dichalcogenide monolayer by large-scale aqueous phase exfoliation to make up for the deficiencies of the prior art.

[0005] Here, we address the important issues mentioned above by developing a versatile combinatorial strategy that enables large-scale delamination of a wide range of TMDs in water without the use of any chemical additives during liquid exfoliation; we use probe ultrasonic cavitation mechanical exfoliation to delaminate pre-intercalated TMD phases in water to produce various TMD monolayers, including MoS2, WS2, MoSe2, WSe2, and ReS2.

[0006] To achieve the above object, the present invention is implemented by the following technical solutions: A method for preparing a transition metal dichalcogenide monolayer by large-scale aqueous exfoliation comprises the following steps: Step 1: Preparation of lithium pre-intercalated TMD powder: (1) Pre-intercalation of TMD crystal powder by immersing it in a n-butyl lithium / hexane solution; (2) After the pre-intercalation is completed, the solution is filtered and washed to recover the lithium-intercalated TMD crystals to obtain lithium-pre-intercalated layered TMD crystals; Step 2: Preparation of water-swelled exfoliated TMD clay-like multilayers: (3) immersing the lithium pre-intercalated layered TMD crystal in deoxygenated deionized water and performing ultrasonic treatment; (4) washing with deionized water and then centrifuging to obtain a TMD clay-like multilayer structure with expanded interlayer water molecules; Step 3: Preparation of aqueous TMD monolayer colloidal dispersion: (5) dispersing the TMD clay-like multilayer in deoxygenated deionized water and exfoliating it using probe ultrasound in an ice bath; (6) Finally, centrifugation is performed and only the supernatant volume is taken as the transition metal dichalcogenide monolayer colloidal dispersion.

[0007] Furthermore, the reaction conditions in step (1) are that the water and oxygen contents are both less than 0.1 ppm, the pre-intercalation reaction time is 3-5 days, and magnetic stirring is continuously performed in an inert gas atmosphere throughout the process.

[0008] Furthermore, the step (2) is carried out in an atmosphere filled with inert gas, and washing is performed using an alkane organic solvent.

[0009] Furthermore, the step (3) is to perform ultrasound in an ice bath: the ultrasound power is 220-260 W, the time is 30-35 min, and the pre-intercalated lithium ions are washed out.

[0010] Furthermore, in step (4), deionized water is used to wash to fully remove the pre-intercalated lithium ions, while allowing water molecules to further intercalate and peel off the TMD multilayers. The centrifugal conditions are: 4000-5000 rpm speed, separation 2-30 min.

[0011] Furthermore, in step (5), the probe ultrasonic stripping time is 30-35 min and the power is 250-300 W.

[0012] Furthermore, in step (6), the centrifugation condition is 3000-4000 rpm for 20-25 min, and it is best to take only 3 / 4 of the volume of the supernatant after centrifugation.

[0013] Application of the transition metal dichalcogenide monolayer prepared by the above method in electronic products.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention uses water as a solvent, which is low in cost and does not use any additives. There is no problem that the added additives will adhere to the surface of the TMD sheet and thus affect its overall performance. The TMD single-sheet yield obtained by the present invention is high, can be prepared on a large scale, and the concentration is higher than 2.5 g L -1 , with high stability, the stability lasts for more than one month.

[0015] The water-dispersed TMDs are initially dominated by the 1T metallic phase, which can be transformed into the 2H semiconductor phase after annealing. The two-dimensional TMDs prepared by the present invention can be mixed with a series of functional materials (including MXene, graphene and nanocellulose) to form a two-dimensional multifunctional heterostructure, which can form a stable colloidal dispersion at high concentrations, which provides a versatile platform for assembling a variety of multifunctional composite materials. This is a huge leap for two-dimensional TMDs because it allows the manufacture of a large number of electronic bulk materials and thin-film electronics in a dry or even wet hydrogel state. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Colloidal dispersions in water of different concentrations, where a is MoS2, b is WSe2, c is MoSe2, d is ReS2, and e is WS2.

[0017] Figure 2 is the zeta potential of various TMD dispersions changing with time.

[0018] Figure 3 Figure 2 shows the atomic force microscope image and thickness distribution diagram of well-dispersed MoS2 flakes, where A is the atomic force microscope image, B is the thickness distribution diagram, and 1, 2, and 3 represent the first position, the second position, and the third position, respectively.

[0019] Figure 4 The prepared MoS2 film and MoS2 / CNF, MoS2 / Graphene, and MoS2 / MXene composite films prepared in a mass ratio of 1:1.

[0020] Figure 5 Typical stress-strain curves of MoS2 film and MoS2 / CNF, MoS2 / Graphene, and MoS2 / MXene composite films prepared in a mass ratio of 1:1. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described below through specific embodiments in conjunction with the accompanying drawings.

[0022] Embodiment 1: The specific preparation steps of a two-dimensional MoS2 monolayer are as follows: Step 1: Prepare lithium pre-intercalated MoS2 powder.

[0023] (A) Pre-intercalation of 1 g MoS2 crystalline powder in 6 ml 2.5 M n-butyl lithium / hexane solution with water and oxygen content less than 0.1 ppm. The pre-intercalation reaction time was 3-5 days with continuous magnetic stirring at 350 rpm. The process was carried out in a glove box filled with inert argon gas.

[0024] (B) After pre-intercalation, the solution was filtered and washed with hexane at least four times to remove excess lithium and organic residues, and the lithium-intercalated MoS2 crystals were recovered. The volume of hexane solution used was approximately 100 ml. This process was carried out in a glove box filled with inert argon gas.

[0025] Step 2: Preparation of water-swelling exfoliated MoS2 clay-like multilayers.

[0026] (A) The lithium pre-intercalated layered MoS2 crystals prepared in step 1 were immersed in 100 ml of oxygen-containing deionized water and ultrasonicated for 30 min in an ice bath to wash out the pre-intercalated lithium ions.

[0027] (B) Wash with deionized water 3-4 times to fully remove the pre-intercalated lithium ions, and allow water molecules to further intercalate and peel off the MoS2 multilayers. Centrifuge at 4500 rpm for 2-30 min to obtain a MoS2 clay-like multilayer structure with expanded interlayer water molecules. It should be noted that the centrifuge tube needs to be shaken by hand for at least two minutes before centrifugation to ensure that the precipitate is evenly dispersed.

[0028] Step 3: Prepare aqueous MoS2 monolayer colloidal dispersion.

[0029] (A) The MoS2 clay-like multilayers prepared in step 2 were dispersed in deionized water and exfoliated using ultrasonic probes in an ice bath. The ultrasonic probe exfoliation time was 30 min, the power was 260 W, and the interval was 4 s on / 2 s off.

[0030] (B) After centrifugation at 3000 rpm for 20 min, only 3 / 4 of the supernatant volume was taken as the final MoS2 monolayer colloidal dispersion.

[0031] like Figure 1 As shown in a, the concentration of the MoS2 dispersion prepared by the present invention is as high as 5.1 g L -1 , and after one month of storage, the Zeta potential hardly changed and the dispersion showed no precipitation or agglomeration (e.g. Figure 2 ), showing high stability. Figure 3 The atomic force microscope image and thickness distribution diagram of MoS2 flakes show that the average thickness of a single-layer MoS2 flake is 1.4 nm. In addition, the MoS2 prepared by the present invention can be dispersed in water and can be mixed with other materials in water to prepare composite materials. Figure 4 The prepared MoS2 film and the MoS2 / CNF, MoS2 / Graphene, and MoS2 / MXene composite films prepared at a mass ratio of 1:1. It can be seen from the figure that the prepared composite film has a smooth surface, uniform thickness, and no cracks. Figure 5 These are typical stress-strain curves of MoS2 film and MoS2 / MXene, MoS2 / CNF, and MoS2 / Graphene composite films prepared in a mass ratio of 1:1. It can be seen from the figure that the MoS2 / CNF composite film has the highest mechanical strength, reaching 178 MPa.

[0032] Embodiment 2: The specific preparation steps of a two-dimensional WSe2 monolayer are as follows: Step 1: Prepare lithium pre-intercalated WSe2 powder.

[0033] (A) 1 g of WSe2 crystal powder was pre-intercalated in 6 ml of 2.5 M n-butyllithium / hexane solution with water and oxygen content less than 0.1 ppm. The pre-intercalation reaction time was 3-5 days with continuous magnetic stirring at 350 rpm. The process was carried out in a glove box filled with inert argon gas.

[0034] (B) After the pre-intercalation, the solution was filtered and washed with hexane at least four times to remove excess lithium and organic residues, and the lithium-intercalated WSe2 crystals were recovered. The volume of hexane solution used was approximately 100 ml. This process was carried out in a glove box filled with inert argon gas.

[0035] Step 2: Preparation of water-swelling exfoliated WSe2 clay-like multilayers.

[0036] (A) The lithium pre-intercalated layered WSe2 crystals prepared in step 1 were immersed in 100 ml of oxygen-containing deionized water and ultrasonicated for 30 min in an ice bath to wash out the pre-intercalated lithium ions.

[0037] (B) Wash with deionized water 3-4 times to fully remove the pre-intercalated lithium ions, and allow water molecules to further intercalate and peel off the WSe2 multilayers. Centrifuge at 4500 rpm for 2-30 min to obtain a WSe2 clay-like multilayer structure with expanded interlayer water molecules. It should be noted that the centrifuge tube needs to be shaken by hand for at least two minutes before centrifugation to ensure that the precipitate is evenly dispersed.

[0038] Step 3: Prepare aqueous WSe2 monolayer colloidal dispersion.

[0039] (A) The WSe2 clay-like multilayer prepared in step 2 was dispersed in deionized water and exfoliated using ultrasonic probe in an ice bath. The ultrasonic probe exfoliation time was 30 min, the power was 260 W, and the interval was 4 s on / 2 s off.

[0040] (B) After centrifugation at 3000 rpm for 20 min, only 3 / 4 of the supernatant volume was taken as the final WSe2 monolayer colloidal dispersion.

[0041] like Figure 1 As shown in a, the concentration of the WSe2 dispersion prepared by the present invention is as high as 2.5 g L -1 , and after one month of storage, the Zeta potential hardly changed and the dispersion showed no precipitation or agglomeration (e.g. Figure 2 As shown), it shows high stability. In addition, the WSe2 prepared by the present invention is a single layer and can be dispersed in water, and can be blended with other materials in water to prepare a composite material.

[0042] Embodiment 3: The specific preparation steps of a two-dimensional MoSe2 monolayer are as follows: Step 1: Prepare lithium pre-intercalated MoSe2 powder.

[0043] (A) Pre-intercalation of 1 g MoSe2 crystal powder in 6 ml 2.5 M n-butyllithium / hexane solution with water and oxygen content less than 0.1 ppm. The pre-intercalation reaction time is 3-5 days with continuous magnetic stirring at 350 rpm. The process is carried out in a glove box filled with inert argon gas.

[0044] (B) After pre-intercalation, the solution was filtered and washed with hexane at least four times to remove excess lithium and organic residues, and the lithium-intercalated MoSe2 crystals were recovered. The volume of hexane solution used was approximately 100 ml. This process was carried out in a glove box filled with inert argon gas.

[0045] Step 2: Preparation of water-swelling exfoliated MoSe2 clay-like multilayers.

[0046] (A) The lithium pre-intercalated layered MoSe2 crystals prepared in step 1 were immersed in 100 ml of oxygen-containing deionized water and ultrasonicated for 30 min in an ice bath to wash out the pre-intercalated lithium ions.

[0047] (B) Wash with deionized water 3-4 times to fully remove the pre-intercalated lithium ions, and allow water molecules to further intercalate and peel off the MoSe2 multilayers. Centrifuge at 4500 rpm for 2-30 min to obtain a MoSe2 clay-like multilayer structure with expanded interlayer water molecules. It should be noted that the centrifuge tube needs to be shaken by hand for at least two minutes before centrifugation to ensure that the precipitate is evenly dispersed.

[0048] Step 3: Prepare aqueous MoSe2 monolayer colloidal dispersion.

[0049] (A) The MoSe2 clay-like multilayer prepared in step 2 was dispersed in deionized water and exfoliated using ultrasonic probe in an ice bath. The ultrasonic probe exfoliation time was 30 min, the power was 260 W, and the interval was 4 s on / 2 s off.

[0050] (B) After centrifugation at 3000 rpm for 20 min, only 3 / 4 of the supernatant volume was taken as the final MoSe2 monolayer colloidal dispersion.

[0051] like Figure 1 As shown in a, the concentration of the MoSe2 dispersion prepared by the present invention is as high as 3.7 g L -1 , and after one month of storage, the Zeta potential hardly changed and the dispersion showed no precipitation or agglomeration (e.g. Figure 2 As shown), it shows high stability. In addition, the MoSe2 prepared by the present invention is a single layer and can be dispersed in water, and can be blended with other materials in water to prepare a composite material.

[0052] Embodiment 4: The specific preparation steps of a two-dimensional ReS2 monolayer are as follows: Step 1: Prepare lithium pre-intercalated ReS2 powder.

[0053] (A) Pre-intercalation of 1 g ReS2 crystalline powder in 6 ml 2.5 M n-butyl lithium / hexane solution with water and oxygen content less than 0.1 ppm. The pre-intercalation reaction time was 3-5 days with continuous magnetic stirring at 350 rpm. The process was carried out in a glove box filled with inert argon gas.

[0054] (B) After the pre-intercalation, the solution was filtered and washed with hexane at least four times to remove excess lithium and organic residues, and the lithium-intercalated ReS2 crystals were recovered. The volume of hexane solution used was approximately 100 ml. This process was carried out in a glove box filled with inert argon gas.

[0055] Step 2: Preparation of water-swelling exfoliated ReS2 clay-like multilayers.

[0056] (A) The lithium pre-intercalated layered ReS2 crystals prepared in step 1 were immersed in 100 ml of oxygen-containing deionized water and ultrasonicated for 30 min in an ice bath to wash out the pre-intercalated lithium ions.

[0057] (B) Wash with deionized water 3-4 times to fully remove the pre-intercalated lithium ions, and allow water molecules to further intercalate and peel off the ReS2 multilayers. Centrifuge at 4500 rpm for 2-30 min to obtain a clay-like multilayer structure of ReS2 with expanded interlayer water molecules. It should be noted that the centrifuge tube needs to be shaken by hand for at least two minutes before centrifugation to ensure that the precipitate is evenly dispersed.

[0058] Step 3: Prepare aqueous ReS2 monolayer colloidal dispersion.

[0059] (A) The water-expanded ReS2 clay-like multilayer obtained in step 2 was dispersed in deionized water and exfoliated using probe ultrasound in an ice bath. The probe ultrasound exfoliation time was 30 min, the power was 260 W, and the interval was 4 s on / 2 s off.

[0060] (B) After centrifugation at 3000 rpm for 20 min, only 3 / 4 of the supernatant volume was taken as the final ReS2 monolayer colloidal dispersion.

[0061] like Figure 1 As shown in a, the concentration of the ReS2 dispersion prepared by the present invention is as high as 3.5 g L -1 , and after one month of storage, the Zeta potential hardly changed and the dispersion showed no precipitation or agglomeration (e.g. Figure 2As shown), it shows high stability. In addition, the ReS2 prepared by the present invention is a single layer and can be dispersed in water, and can be blended with other materials in water to prepare a composite material.

[0062] Embodiment 5: The specific preparation steps of a two-dimensional WS2 monolayer are as follows: Step 1: Prepare lithium pre-intercalated WS2 powder.

[0063] (A) 1 g of WS2 crystal powder was pre-intercalated in 6 ml of 2.5 M n-butyllithium / hexane solution with water and oxygen content less than 0.1 ppm. The pre-intercalation reaction time was 3-5 days with continuous magnetic stirring at 350 rpm. The process was carried out in a glove box filled with inert argon gas.

[0064] (B) After the pre-intercalation, the solution was filtered and washed with hexane at least four times to remove excess lithium and organic residues, and the lithium-intercalated WS2 crystals were recovered. The volume of hexane solution used was approximately 100 ml. This process was carried out in a glove box filled with inert argon gas.

[0065] Step 2: Preparation of water-swelling exfoliated WS2 clay-like multilayers.

[0066] (A) The lithium pre-intercalated layered WS2 crystals prepared in step 1 were immersed in 100 ml of oxygen-containing deionized water and ultrasonicated for 30 min in an ice bath to wash out the pre-intercalated lithium ions.

[0067] (B) Wash with deionized water 3-4 times to fully remove the pre-intercalated lithium ions, and allow water molecules to further intercalate and peel off the WS2 multilayers. Centrifuge at 4500 rpm for 2-30 min to obtain a WS2 clay-like multilayer structure with expanded interlayer water molecules. It should be noted that the centrifuge tube needs to be shaken by hand for at least two minutes before centrifugation to ensure that the precipitate is evenly dispersed.

[0068] Step 3: Prepare aqueous WS2 monolayer colloidal dispersion.

[0069] (A) The WS2 clay-like multilayers prepared in step 2 were dispersed in deionized water and exfoliated using ultrasonic probes in an ice bath. The ultrasonic probe exfoliation time was 30 min, the power was 260 W, and the interval was 4 s on / 2 s off.

[0070] (B) After centrifugation at 3000 rpm for 20 min, only 3 / 4 of the supernatant volume was taken as the final WS2 monolayer colloidal dispersion.

[0071] like Figure 1As shown in a, the concentration of the WS2 dispersion prepared by the present invention is as high as 9.5 g L -1 , and after one month of storage, the Zeta potential hardly changed and the dispersion showed no precipitation or agglomeration (e.g. Figure 2 In addition, the WS2 prepared by the present invention is a single layer and can be dispersed in water, and can be blended with other materials in water to prepare a composite material.

[0072] Embodiment 6: The specific preparation steps of a MoS2 / CNF composite film are as follows: The obtained MoS2 dispersion and 1wt% CNF aqueous dispersion were mixed into a uniform dispersion at a mass ratio of MoS2:CNF of 1:1. After vacuum filtration, the mixture was vacuum dried in a vacuum heating dryer at -1 bar and 90°C for 15 min and peeled off from the filter membrane to obtain an independent self-supporting MoS2 / CNF composite film.

[0073] The MoS2 / CNF composite film prepared in Example 6 with a mass ratio of MoS2:CNF of 1:1 has a smooth surface, uniform thickness and no cracks (such as Figure 4 The composite film thickness is about 10 μm and the mechanical strength is as high as 178 MPa (as shown in Figure 5 as shown).

[0074] Embodiment 7: The specific preparation steps of a MoS2 / Graphene composite film are as follows: The obtained MoS2 dispersion and the concentration of 1 g L -1 The graphene aqueous dispersion was prepared into a uniformly mixed dispersion according to the mass ratio of MoS2:Graphene of 1:1. After vacuum filtration, it was vacuum dried in a vacuum heating dryer at -1 bar and 90°C for 15 min and peeled off from the filter membrane to obtain an independent self-supporting MoS2 / Graphene composite film.

[0075] The independent self-supporting MoS2 / Graphene composite film with a mass ratio of MoS2:Graphene of 1:1 prepared in Example 7 has a smooth surface, uniform thickness and no cracks (such as Figure 4 The composite film thickness is about 10 μm and the mechanical strength is 15 MPa (as shown in Figure 5 as shown).

[0076] Embodiment 8: The specific preparation steps of a MoS2 / MXene composite film are as follows: The obtained MoS2 dispersion and the concentration of 1 g L -1 The MXene aqueous dispersion was prepared into a uniformly mixed dispersion according to the mass ratio of MoS2:MXene of 1:1. After vacuum filtration, it was vacuum dried in a vacuum heating dryer at -1 bar and 90 °C for 15 min and peeled off from the filter membrane to obtain an independent self-supporting MoS2 / MXene composite film.

[0077] The independent self-supporting MoS2 / MXene composite film with a mass ratio of MoS2:MXene of 1:1 prepared in Example 8 has a smooth surface, uniform thickness and no cracks (such as Figure 4 The composite film thickness is about 10 μm and the mechanical strength is as high as 69.71 MPa (as shown in Figure 5 as shown).

[0078] It can be seen from the above examples that: The two-dimensional TMD prepared by the present invention can be mixed with a series of functional materials (including MXene, graphene and nanocellulose), can form a stable colloidal dispersion at high concentration, and can be assembled into various multifunctional independent self-supporting composite film materials in a dry or even wet hydrogel state, which provides a multifunctional platform for assembling various multifunctional composite materials. The prepared independent self-supporting composite film is only about 10 μm thick, and the surface of the composite film is flat, the thickness is uniform, and there are no cracks. The mechanical strength of the MoS2 / Graphene composite film is 15 MPa, and the mechanical strength of the MoS2 / MXene composite film is as high as 69.71 MPa. Compared with other composite films, the MoS2 / CNF composite film exhibits the highest mechanical strength of 178 MPa. This provides a variety of possibilities for the application of 2D TMD nanocomposites in flexible electronics, soft robots and energy storage.

[0079] Finally, although this specification is described according to implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A method for preparing a transition metal dichalcogenide monolayer by large-scale aqueous exfoliation, characterized in that: The method comprises the following steps: (1) Pre-intercalation of TMD crystal powder by immersing it in a n-butyl lithium / hexane solution; (2) After the pre-intercalation is completed, the solution is filtered and washed to recover the lithium-intercalated TMD crystals to obtain lithium-pre-intercalated layered TMD crystals; (3) immersing the lithium pre-intercalated layered TMD crystal in deoxygenated deionized water and performing ultrasonic treatment; (4) washing with deionized water and then centrifuging to obtain a TMD clay-like multilayer structure with expanded interlayer water molecules; (5) dispersing the TMD clay-like multilayer in deoxygenated deionized water and exfoliating it using probe ultrasound in an ice bath; (6) Finally, centrifugation is performed and only the supernatant volume is taken as the transition metal dichalcogenide monolayer colloidal dispersion.

2. The method for preparing a transition metal dichalcogenide monolayer by aqueous large-scale exfoliation according to claim 1, characterized in that: The reaction conditions in step (1) are that the water and oxygen contents are both less than 0.1 ppm, the pre-intercalation reaction time is 3-5 days, and magnetic stirring is performed continuously, and the whole process is carried out in an atmosphere filled with inert gas.

3. The method for preparing a transition metal dichalcogenide monolayer by aqueous large-scale exfoliation according to claim 1, characterized in that: The step (2) is carried out in an atmosphere filled with inert gas, and washing is performed using an alkane organic solvent.

4. The method for preparing a transition metal dichalcogenide monolayer by aqueous large-scale exfoliation according to claim 1, characterized in that: The step (3) is to perform ultrasound in an ice bath: the ultrasound power is 220-260 W, the time is 30-35 min, and the pre-intercalated lithium ions are washed out.

5. The method for preparing a transition metal dichalcogenide monolayer by aqueous large-scale exfoliation according to claim 1, characterized in that: In the step (4), deionized water is used to wash to fully remove the pre-intercalated lithium ions, while allowing water molecules to further intercalate and peel off the TMD multilayers. The centrifugal conditions are: 4000-5000 rpm speed, separation 2-30 min.

6. The method for preparing a transition metal dichalcogenide monolayer by aqueous large-scale exfoliation according to claim 1, characterized in that: In the step (5), the probe ultrasonic stripping time is 30-35 min, and the power is 250-300 W.

7. The method for preparing a transition metal dichalcogenide monolayer by aqueous large-scale exfoliation according to claim 1, characterized in that: In the step (6), the centrifugation condition is 3000-4000 rpm for 20-25 min, and it is best to take only 3 / 4 of the volume of the supernatant after centrifugation.

8. Application of the transition metal dichalcogenide monolayer prepared by the method of claim 1 in electronic products.

Citation Information

Patent Citations

  • Method for preparing molybdenum disulfide nanosheets by ultrasonic-assisted chemical intercalation

    CN104310482A

  • Liquid-phase peeling method for transition metal disulphide nanosheets

    CN106966371A