Basalt-based whisker composite material and preparation method thereof

By introducing silicon carbide, zinc oxide and calcium sulfate whiskers into the basalt glass matrix, the basalt-based whisker composite material is formed, which solves the problem of insufficient toughness of the basalt material, and achieves the maintenance of wear resistance, corrosion resistance and high temperature resistance while maintaining wear resistance, corrosion resistance and high temperature resistance. Improve material toughness.

CN118930060APending Publication Date: 2024-11-12CHENGDU UNIV OF INFORMATION TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411177177.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Basalt materials have poor toughness, which makes them fragile during collisions and bumps, limiting their widespread application and it is difficult to maintain wear-resistant, corrosion-resistant and high-temperature-resistant properties when improving toughness.

Method used

Silicon carbide whiskers, zinc oxide whiskers and calcium sulfate whiskers are introduced into the basalt glass matrix, and they are evenly distributed through the sintering process to form a basalt-based whisker composite material to improve the toughness of the material.

Benefits of technology

It effectively improves the toughness of basalt materials, while maintaining wear-resistant, corrosion-resistant and high-temperature resistance. Through crack bridge, deflection and pull-out effects, the composite material can absorb and consume stress more under external stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011019960000081
    Figure BDA0005011019960000081
Patent Text Reader

Abstract

The invention discloses a basalt-based whisker composite material and a preparation method thereof.The basalt-based whisker composite material comprises a basalt glass matrix and whiskers distributed in the basalt glass matrix, and the whiskers are selected from at least one of silicon carbide whiskers, zinc oxide whiskers and calcium sulfate whiskers. The mass fraction of crystal whiskers in the basalt-based crystal whisker composite material is 1%-25%. At least one of the silicon carbide whiskers, the zinc oxide whiskers and the calcium sulfate whiskers is introduced into a basalt glass matrix, the whiskers can resist high temperature and wear and are low in thermal expansion coefficient, and after the whiskers are doped, when the composite material is subjected to external stress, due to the crack bridging principle, the crack deflection principle, the pull-out effect and the like, the thermal expansion coefficient of the composite material is greatly improved. The crystal whiskers uniformly distributed in the basalt can absorb and consume stress, so that the toughness of the matrix material can be effectively improved, and the toughness of the material is improved while the wear resistance, corrosion resistance, high temperature resistance and other properties of the basalt material are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of basalt materials, in particular to a basalt-based whisker composite material and a preparation method thereof. Background Art

[0002] Basalt is a rock formed by the cooling of natural volcanic rock after melting. Its main component is SiO 2 、Al 2 O 3 In addition, it also contains a small amount of Fe 2 O 3 / FeO, CaO, MgO, TiO 2 、Na 2 O / Ka 2 O, etc. Due to different regions, the internal composition of the mined basalt is slightly different. In the past 100 years of development, basalt products such as basalt fiber, basalt rock wool, and basalt cast stone have been discovered. However, the direct products produced by basalt have the disadvantages of poor toughness, high processing difficulty, high hardness and difficulty in making parts. Therefore, improving its toughness and making this low-cost, simple to make, excellent in performance, safe and environmentally friendly material more widely used in our lives has become an important research direction.

[0003] Basalt glass is a material that can be obtained by melting basalt after high-temperature calcination and cooling. You can get the desired parts through molds, cutting and grinding. It has good plasticity when molten, and has the advantages of wear resistance, corrosion resistance, high temperature resistance, low cost, and low density. It is often used in automotive interior decoration, bottom device parts, muffler and towing system, radiator parts, metal coating, etc. However, whether it is glass basalt or crystallized basalt, it is a brittle material with poor toughness. It is easy to break when encountering collisions and bumps when it is in glass state and cast stone, which will affect people's life and property safety. Therefore, it has certain limitations in use, which affects its widespread use.

[0004] Some studies have woven fibers into fiber cloth, and then bonded the fiber cloth together with adhesives for many times. The material formed in this way can replace the work of basalt glass and cast stone, and it is also a relatively mature technology to modify and toughen the fiber surface. However, there are inevitable gaps in basalt fiber cloth during weaving. If it is filled with other high-temperature materials or wear-resistant materials, the cost will inevitably increase, and the overall wear resistance and corrosion resistance will decrease. In view of this, it is particularly necessary to improve the toughness of basalt materials while ensuring their wear resistance, corrosion resistance, high temperature resistance and other properties. Summary of the invention

[0005] The object of the present invention is to provide a basalt-based whisker composite material and a preparation method thereof, which can improve the toughness of the material while ensuring the wear resistance, corrosion resistance, high temperature resistance and other properties of the basalt material.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a basalt-based whisker composite material, comprising a basalt glass matrix and whiskers distributed in the basalt glass matrix, wherein the whiskers are selected from at least one of silicon carbide whiskers, zinc oxide whiskers and calcium sulfate whiskers, and the mass fraction of the whiskers in the basalt-based whisker composite material is 1% to 25%.

[0008] In an optional embodiment, the whiskers have an average diameter of 0.4 μm to 1 μm and an average length of 5 μm to 16 μm.

[0009] In a second aspect, the present invention provides a method for preparing the basalt-based whisker composite material as described in any one of the aforementioned embodiments, comprising: sintering a mixture of basalt sand and whiskers to obtain the basalt-based whisker composite material.

[0010] In an optional embodiment, the sintering temperature is 900° C. to 1300° C., the sintering time is 0.5 h to 6 h, and the sintering pressure is 50 MPa to 500 MPa.

[0011] In an optional embodiment, the heating rate before sintering is 2°C / min to 5°C / min;

[0012] And / or, the cooling rate after sintering is 2°C / min to 5°C / min.

[0013] In an optional embodiment, the preparation method of the mixture includes: mixing basalt sand with a dispersion liquid in which whiskers are dispersed, and then drying to obtain the mixture;

[0014] Preferably, the mass fraction of the solvent in the mixture is less than 62%.

[0015] In an optional embodiment, the dispersion comprises ethanol, polyethylene glycol and water, the mass ratio of ethanol, polyethylene glycol and water in the dispersion is 25:1, and the water content in the dispersion is less than 2wt%;

[0016] In an optional embodiment, the method for preparing the dispersion includes: adding whiskers to a prepared dispersion, and mixing the mixture to obtain the dispersion containing the whiskers.

[0017] In an optional embodiment, the solid content of the dispersion containing the whiskers is (0.2-5) g / (20-50) ml.

[0018] In an optional embodiment, the mixing step is accompanied by ultrasound and stirring, the ultrasound time is 10 min to 30 min, the stirring time is 10 min to 30 min, and the stirring speed is 300 min to 500 r / min.

[0019] The present invention has the following beneficial effects:

[0020] The basalt-based whisker composite material provided by the present invention introduces at least one of silicon carbide whiskers, zinc oxide whiskers and calcium sulfate whiskers into a basalt glass matrix. The whiskers themselves are resistant to high temperatures, wear-resistant and have a low thermal expansion coefficient. After the whiskers are doped, when the composite material is subjected to external stress, due to the crack bridging principle, crack deflection principle and pull-out effect, the whiskers evenly distributed in the basalt will absorb and consume stress, which can effectively improve the toughness of the matrix material, so as to improve the toughness of the material while ensuring the wear resistance, corrosion resistance, high temperature resistance and other properties of the basalt material. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0022] An embodiment of the present invention provides a basalt-based whisker composite material, comprising a basalt glass matrix and whiskers distributed in the basalt glass matrix, wherein the whiskers are selected from at least one of silicon carbide whiskers, zinc oxide whiskers and calcium sulfate whiskers, and the mass fraction of the whiskers in the basalt-based whisker composite material is 1% to 25%.

[0023] The basalt-based whisker composite material provided in the embodiment of the present invention introduces at least one of silicon carbide whiskers, zinc oxide whiskers and calcium sulfate whiskers into a basalt glass matrix. The whiskers themselves can be resistant to high temperatures, wear-resistant, and have a low thermal expansion coefficient. After the whiskers are doped, when the composite material is subjected to external stress, due to the crack bridging principle, crack deflection principle and pull-out effect, the whiskers evenly distributed in the basalt will absorb and consume stress, which can effectively improve the toughness of the matrix material, so as to improve the toughness of the material while ensuring the wear resistance, corrosion resistance, high temperature resistance and other properties of the basalt material.

[0024] In the present invention, the mass fraction of whiskers in the basalt-based whisker composite material is 1% to 25%, specifically 1%, 5%, 10%, 15%, 20%, 25% or any value between 1% and 25%. If the amount of whiskers added is too little, the effect of improving toughness is not obvious, but if the amount of whiskers added is too much, it may cause changes in the performance of the basalt glass matrix, resulting in a significant reduction in properties such as wear resistance, corrosion resistance, and high temperature resistance.

[0025] In an optional embodiment, the average diameter of the whiskers is 0.4 μm to 1 μm, specifically 0.4 μm, 0.6 μm, 0.8 μm, 1 μm or any value between 0.4 μm and 1 μm; the average length is 5 μm to 16 μm, specifically 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm or any value between 5 μm and 16 μm.

[0026] When the whisker size is too large, the total contact area between the whisker and the basalt glass matrix is ​​reduced. According to the pull-out effect, the presence of the whisker reduces the toughness effect of the basalt glass matrix. Similarly, when the whisker size is too small, the contact area between a single whisker and the basalt glass matrix is ​​reduced, which reduces the stress that needs to be overcome during the whisker pull-out process, thereby reducing the toughness effect of the whisker on the basalt glass matrix.

[0027] An embodiment of the present invention further provides a method for preparing the basalt-based whisker composite material as described in any one of the aforementioned embodiments, comprising: sintering a mixture of basalt sand and whiskers to obtain the basalt-based whisker composite material.

[0028] The preparation method of the basalt-based whisker composite material of the present embodiment is simple, and only requires that the basalt sand and the whiskers be uniformly mixed and then sintered so that the basalt glass matrix and the whiskers are in full contact with each other.

[0029] In an optional embodiment, the sintering temperature is 900° C. to 1300° C., the sintering time is 0.5 h to 6 h, and the sintering pressure is 50 MPa to 500 MPa.

[0030] During the sintering process, the basalt sand is melted to obtain a basalt glass matrix, and the whiskers are relatively evenly dispersed in the matrix.

[0031] In the embodiment of the present invention, the sintering temperature is 900° C. to 1300° C., and the substrate temperature can be 900° C., 1000° C., 1100° C., 1200° C., 1300° C. or any value between 900° C. and 1300° C., preferably 1100° C. to 1300° C. If the sintering temperature is too high, the whiskers may react with some components in the basalt glass matrix, thereby reducing the effect of improving the toughness of the material.

[0032] In the embodiment of the present invention, in order to minimize or even avoid the reaction between the basalt glass matrix and the whiskers, the sintering pressure is increased. Specifically, the sintering pressure can be 50MPa, 100MPa, 200MPa, 300MPa, 400MPa, 500MPa or any value between 50MPa and 500MPa. Pressurization is beneficial to lowering the melting point of basalt sand, thereby lowering the sintering temperature.

[0033] The sintering time can be 0.5h to 6h, specifically 0.5h, 1h, 2h, 3h, 4h, 5h, 6h or any value between 0.5h and 6h, to ensure that the basalt sand is melted and in full contact with the whiskers.

[0034] In an optional embodiment, the heating rate before sintering is 2°C / min to 5°C / min, specifically 2°C / min, 3°C / min, 4°C / min, 5°C / min or any value between 2°C / min and 5°C / min.

[0035] In an optional embodiment, the cooling rate after sintering is 2°C / min to 5°C / min, specifically 2°C / min, 3°C / min, 4°C / min, 5°C / min or any value between 2°C / min and 5°C / min.

[0036] Both the heating rate and the cooling rate will affect the degree of improvement in the toughness of the basalt glass matrix.

[0037] In an optional embodiment, the preparation method of the mixture includes: mixing basalt sand with a dispersion liquid in which whiskers are dispersed, and then drying to obtain the mixture;

[0038] Preferably, the mass fraction of the solvent in the mixture is less than 62%.

[0039] Mixing basalt sand and whiskers in the presence of a dispersion liquid is conducive to uniform mixing of the two. It should be noted that in order to improve the uniformity of whisker dispersion in the basalt glass matrix, the basalt sand and whiskers in the mixture also need to be uniformly mixed. Therefore, the particle size of the basalt sand should not be too large. Usually, the particle size of the basalt sand is about 400 μm.

[0040] In an optional embodiment, the dispersion comprises ethanol, polyethylene glycol and water, the mass ratio of ethanol, polyethylene glycol and water in the dispersion is 25:1, and the water content in the dispersion is less than 2wt%;

[0041] The presence of the dispersion liquid is beneficial to promoting the uniform distribution of the whiskers in the basalt sand and inhibiting the agglomeration of the whiskers.

[0042] In an optional embodiment, the method for preparing the dispersion includes: adding whiskers to a prepared dispersion, and mixing the mixture to obtain the dispersion containing the whiskers.

[0043] In an optional embodiment, the solid content of the dispersion containing the whiskers is (0.2-5) g / (20-50) ml, which is conducive to uniform mixing of the whiskers and the basalt sand.

[0044] In an optional embodiment, the mixing step is accompanied by ultrasound and stirring, the ultrasound time is 10 min to 30 min, the stirring time is 10 min to 30 min, and the stirring speed is 300 min to 500 r / min. Ultrasound and stirring are combined to improve the uniformity of the mixture.

[0045] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0046] Example 1

[0047] This embodiment provides a method for preparing a basalt-based whisker composite material, which specifically includes:

[0048] Adding silicon carbide whiskers to a dispersion and mixing them to obtain a dispersion with a solid content of 0.04878 g / ml; wherein the average diameter of the whiskers is 0.5 μm, the average length is 12 μm, the mass ratio of ethanol to polyethylene glycol in the dispersion is 25:1, and the water content in the dispersion is less than 2 wt %; the mixing process is accompanied by ultrasound and stirring, the ultrasound time is 20 min, the stirring time is 20 min, and the stirring speed is 400 r / min;

[0049] Adding basalt sand to the dispersion, mixing evenly and then drying to obtain a mixture, wherein the mass fraction of whiskers in the mixture is 10%; the mixing process is accompanied by ultrasound and stirring, wherein the ultrasound time is 20 minutes, the stirring time is 20 minutes, and the stirring speed is 400 r / min;

[0050] The mixture is sintered at a sintering temperature of 1100° C., a sintering time of 40 min, a sintering pressure of 450 MPa, a heating rate of 2° C. / min to 5° C. / min, and a cooling rate of 2° C. / min to 5° C. / min.

[0051] Example 2

[0052] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the sintering temperature is 900°C.

[0053] Example 3

[0054] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the sintering temperature is 1300°C.

[0055] Example 4

[0056] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the sintering pressure is 50 MPa.

[0057] Example 5

[0058] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the sintering pressure is 500 MPa.

[0059] Example 6

[0060] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the mass fraction of the whiskers in the mixture is 1%.

[0061] Example 7

[0062] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the mass fraction of whiskers in the mixture is 25%.

[0063] Example 8

[0064] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the whiskers are replaced with zirconium oxide whiskers.

[0065] Example 9

[0066] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the whiskers are replaced with zirconium boride whiskers.

[0067] Example 10

[0068] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the sintering temperature is 1450° C. and the sintering pressure is 0.1 MPa.

[0069] Embodiment 11

[0070] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that the sintering pressure is 0.1 MPa.

[0071] Comparative Example 1

[0072] This embodiment provides a method for preparing a basalt-based whisker composite material, which is different from Embodiment 1 only in that whiskers are not added to the dispersion.

[0073] The properties of the basalt-based whisker composite materials prepared in the above examples and comparative examples were tested, and the results are shown in Table 1.

[0074] Table 1

[0075]

[0076]

[0077] In the present application, too low a temperature will affect the melting of basalt to form a glassy state. If there are unmelted substances inside, it will affect its various properties. Too high a temperature will cause a reaction between whiskers and basalt.

[0078] If high pressure is not applied, the sintering temperature of basalt glass is about 1300℃, which will cause whiskers to react with basalt, thus losing the purpose of enhancing performance. Applying high pressure can reduce the sintering temperature and increase the density of glass, but the effect is not obvious if the pressure is too low.

[0079] If the whisker content is too large, the whiskers will aggregate and the bonding between the whiskers and the basalt will decrease, thus reducing its performance. If the whisker content is too low, it will not be enough to absorb external stress, and the performance enhancement effect will not be obvious.

[0080] In the present application, different types of whiskers have different binding properties with basalt, and different whiskers have different high temperature resistance. Different whiskers also enhance different properties. For example, silicon carbide whiskers can enhance the high temperature resistance, wear resistance, and toughness of composite materials.

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A basalt-based whisker composite material, characterized in that: The composite material comprises a basalt glass matrix and whiskers distributed in the basalt glass matrix. The whiskers are selected from at least one of silicon carbide whiskers, zinc oxide whiskers and calcium sulfate whiskers. The mass fraction of the whiskers in the basalt-based whisker composite material is 1% to 25%.

2. The basalt-based whisker composite material according to claim 1, characterized in that: The average diameter of the whiskers is 0.4 μm to 1 μm, and the average length is 5 μm to 16 μm.

3. A method for preparing the basalt-based whisker composite material according to any one of claims 1 to 2, characterized in that: include: The mixture of basalt sand and whiskers is sintered to obtain the basalt-based whisker composite material.

4. The method for preparing the basalt-based whisker composite material according to claim 3, characterized in that: The sintering temperature is 900° C. to 1300° C., the sintering time is 0.5 h to 6 h, and the sintering pressure is 50 MPa to 500 MPa.

5. The method for preparing the basalt-based whisker composite material according to claim 3, characterized in that: The heating rate before sintering is 2℃ / min~5℃ / min; And / or, the cooling rate after sintering is 2°C / min to 5°C / min.

6. The method for preparing the basalt-based whisker composite material according to claim 3, characterized in that: The preparation method of the mixture comprises: mixing basalt sand with a dispersion liquid in which whiskers are dispersed, and then drying to obtain the mixture; Preferably, the mass fraction of the solvent in the mixture is less than 62%.

7. The method for preparing the basalt-based whisker composite material according to claim 6, characterized in that: The dispersion liquid comprises ethanol, polyethylene glycol and water, the mass ratio of ethanol to polyethylene glycol in the dispersion liquid is 25:1, and the water content in the dispersion liquid is less than 2wt%.

8. The method for preparing the basalt-based whisker composite material according to claim 6, characterized in that: The preparation method of the dispersion comprises: adding whiskers into a prepared dispersion, and mixing the mixture to obtain the dispersion containing the whiskers.

9. The method for preparing the basalt-based whisker composite material according to claim 6, characterized in that: The solid content of the dispersion containing the whiskers is (0.2-5) g / (20-50) ml.

10. The method for preparing the basalt-based whisker composite material according to any one of claims 6 to 9, characterized in that: The mixing step is accompanied by ultrasound and stirring, the ultrasound time is 10 min to 30 min, the stirring time is 10 min to 30 min, and the stirring speed is 300 min to 500 r / min.

Citation Information

Patent Citations

  • Armor material and method for producing it

    CN101285667A

  • Basalt fiber based on zirconia phase change toughening and preparation method thereof

    CN118439790A