Manufacturing method of ultra-high performance rubber concrete
By using technical means such as rubber particles and nanomaterials in ultra-high performance concrete, the problem of insufficient tensile and crack resistance of traditional ultra-high performance concrete is solved, and higher tensile and compressive strength and durability are achieved. for high demands in building and infrastructure projects.
Patent Information
- Application Number
- CN202411051301.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional ultra-high performance concrete has shortcomings in tensile and crack resistance and cannot meet the requirements of certain application environments.
Using a method of making ultra-high performance rubber concrete, by selecting appropriate raw materials such as silicate cement, microsilicon powder, quartz powder, quartz sand, rubber particles and nanomaterials, and through specific stirring, pouring and curing processes, Including rubber particle surface treatment, vacuum defoaming, ultrasonic treatment and microwave curing to improve the toughness, compressive strength, wear resistance and durability of concrete.
The tensile and crack resistance of concrete is significantly improved, its ductility under tensile stress and load bearing capacity under compressive stress, improve wear resistance and durability, and accelerate construction progress.
Smart Images

Figure CN118930176A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete production, and in particular to a method for producing ultra-high performance rubber concrete. Background Art
[0002] In recent years, with the continuous improvement of material performance requirements in modern construction and infrastructure projects, ultra-high performance concrete (UHPC), as a new type of high-performance building material, has attracted extensive attention and research due to its excellent mechanical properties and durability.
[0003] However, traditional ultra-high performance concrete mainly relies on materials such as cement, silica fume and quartz powder, which may have certain limitations in certain application environments, such as insufficient toughness, poor tensile and crack resistance, etc. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing ultra-high performance rubber concrete, which solves the problem that traditional ultra-high performance concrete has poor tensile and crack resistance.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A method for preparing ultra-high performance rubber concrete, comprising the following specific steps:
[0006] S1: Material preparation, selecting silicate cement, microsilica powder, quartz powder, quartz sand, rubber particles, water and water reducing agent as raw materials;
[0007] S2: Material weighing: use an electronic scale to weigh each raw material separately, and use a separate container to hold each material;
[0008] S3: Dry mixing: put high-grade cement, silica fume and quartz powder into a mixer according to the proportion, stir at low speed for 2-5 minutes, then stir at high speed for 2-5 minutes, then add quartz sand, stir at low speed for 1-3 minutes, and stir at high speed for 2-4 minutes;
[0009] S4: Add rubber particles. During the stirring process, gradually add rubber particles, stir at a low speed for 2-5 minutes, and then stir at a high speed for 4-8 minutes;
[0010] S5: Wet mixing, continue mixing until the concrete is uniform and there are no dry powder lumps, the total mixing time is controlled within 5-10 minutes, and use a scraper to scrape the mixture on the mixer wall regularly;
[0011] S6: Surface treatment of rubber particles: put the rubber particles into a container, add an appropriate amount of silane coupling agent solution, which is a 1:10 dilution of the coupling agent and water, soak for 20-40 minutes, take out the rubber particles, and dry them for later use;
[0012] S7: Casting and molding: pour the evenly mixed concrete into the mold, vibrate the mold with a vibrator to expel bubbles, and control the vibration time to 1-4 minutes. During the vibration process, observe whether there are bubbles escaping from the mold surface;
[0013] S8: Curing: standard curing is carried out after pouring is completed. Curing is carried out for 25-30 days at 20℃-25℃ and relative humidity of 90%-100%. Keep it moist during curing, cover it with wet linen or spray it with curing liquid.
[0014] Preferably, the silicate cement in step S1 is selected from grade 52.5 silicate cement, the particle size of microsilica powder is 0.1-1 micron, the particle size of quartz powder is 10-100 micron, the particle size of quartz sand is 0.1-2 mm, and the particle size of rubber particles is 0.5-2 mm. In step S2, high-grade cement accounts for 45%-55%, silica fume accounts for 5%-10%, quartz powder accounts for 10%-15%, quartz sand accounts for 25%-35%, rubber particles account for 5%-10%, and the water-cement ratio is 0.20-0.25, that is, the mass of water is 20%-25% of the total mass of cement, silica fume and quartz powder, and the water reducer accounts for 0.8%-1.5% of the mass of cement.
[0015] Preferably, after the step S3, water, a water reducing agent and a plasticizer are gradually added to the dry mixture, and the mixture is first stirred at a low speed for 3-6 minutes to allow the water and the powder to fully contact, and then stirred at a high speed for 3-6 minutes.
[0016] Preferably, the plasticizer is 0.5%-1% of the mass of cement.
[0017] Preferably, after the step S3, fibers are gradually added to the wet mixture, stirred at a low speed for 2-5 minutes, and then stirred at a high speed for 3-6 minutes to completely mix the fibers into the concrete.
[0018] Preferably, the fiber accounts for 0.5%-2%.
[0019] Preferably, after the step S5, the mixed concrete is placed in a vacuum device for vacuum degassing to remove bubbles in the concrete for 10-15 minutes.
[0020] Preferably, after the vacuum degassing, the concrete is treated with ultrasonic equipment for 5-10 minutes.
[0021] Preferably, after ultrasonic treatment, 0.5% to 2% of the total mass of nanomaterials are added, the nanomaterials include nano-silicon dioxide, and stirred at a low speed for 2-5 minutes and at a high speed for 3-8 minutes.
[0022] Preferably, after the step S7, the concrete is cured using microwave equipment after casting to accelerate the initial and final setting of the concrete, and the time is 15-20 minutes.
[0023] The present invention provides a method for producing ultra-high performance rubber concrete, which has the following beneficial effects:
[0024] 1. The present invention increases the toughness of concrete through rubber particles, so that it has better ductility under tensile stress, reduces the generation and expansion of cracks, and polypropylene fibers or steel fibers can effectively disperse tensile stress and further enhance the crack resistance of concrete, thereby achieving the effect of improving the tensile and crack resistance of the concrete.
[0025] 2. The present invention improves the overall strength of concrete by using high-grade cement and silica fume, so that it can withstand higher compressive stress. After sufficient mixing and vibration, the concrete structure is denser and the internal pores are reduced, thereby achieving the effect of improving the compressive strength of concrete.
[0026] 3. The present invention increases the surface wear resistance of concrete through rubber particles, and is suitable for use in high-wear environments. The elasticity and toughness of rubber can buffer the damage to the concrete structure caused by temperature changes and enhance its durability. The addition of rubber particles enables concrete to have better chemical corrosion resistance in acidic and alkaline environments, thereby achieving the effect of improving the durability of the concrete.
[0027] 4. The present invention improves the microstructure of concrete by adding 0.5%-2% of nanomaterials, thereby achieving the effect of improving the mechanical properties of the concrete.
[0028] 5. The present invention accelerates the initial setting and final setting of concrete through microwave curing treatment, improves early strength, and thus can achieve the effect of accelerating the construction progress. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The present invention is a flow chart of the method for making ultra-high performance rubber concrete. DETAILED DESCRIPTION
[0030] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] Please refer to the attached Figure 1The present invention provides a method for preparing ultra-high performance rubber concrete, comprising the following specific steps:
[0033] S1: Material preparation, select silicate cement, microsilica powder, quartz powder, quartz sand, rubber particles, water and water reducing agent as raw materials for subsequent operations;
[0034] S2: Material weighing: use an electronic scale to weigh each raw material separately, and use a separate container to hold each material;
[0035] S3: Dry mixing: put high-grade cement, silica fume and quartz powder into a mixer according to the proportion, stir at low speed for 2 minutes to ensure preliminary mixing, then stir at high speed for 3 minutes to make the mixture uniform, add quartz sand, stir at low speed for 2 minutes, and stir at high speed for 3 minutes to ensure uniform distribution of each component;
[0036] S4: Add rubber particles. During the mixing process, gradually add the rubber particles and stir at a low speed for 2 minutes to disperse the rubber particles in the mixture, and then stir at a high speed for 5 minutes to ensure that the rubber particles are evenly distributed in the concrete;
[0037] S5: Wet mixing, continue mixing until the concrete is uniform and there are no dry powder lumps. The total mixing time is controlled within 5-10 minutes. Use a scraper or other tools to regularly scrape the mixture on the mixer wall to ensure that all materials are evenly mixed;
[0038] S6: Surface treatment of rubber particles. In order to improve the bonding performance between rubber particles and cement substrate, the rubber particles can be surface treated, for example, using silane coupling agent to treat the rubber particles, or roughening the surface of the rubber particles. Put the rubber particles in a container, add an appropriate amount of silane coupling agent solution - a 1:10 dilution of coupling agent and water, soak for 30 minutes, take out the rubber particles, dry them and set aside;
[0039] S7: Casting and molding. Pour the evenly mixed concrete into the mold, vibrate the mold with a vibrator to expel bubbles and improve the density of the concrete. The vibration time is controlled within 1-2 minutes. During the vibration process, observe whether there are bubbles escaping from the mold surface to ensure that there are no large bubbles inside the concrete.
[0040] S8: Curing. After pouring, standard curing is carried out at 20°C and relative humidity above 90% for 28 days to achieve the designed strength. Keep it moist during the curing period, cover it with wet burlap or spray it with curing liquid. Check the moisture content of the concrete regularly to avoid cracking of the concrete surface due to water loss.
[0041] The silicate cement in step S1 is selected to be 52.5 grade silicate cement, the particle size of microsilica powder is 0.1-1 micron, the particle size of quartz powder is 10-100 micron, the particle size of quartz sand is 0.1-2 mm, and the particle size of rubber particles is 0.5-2 mm. In step S2, high-grade cement accounts for 50%, silica fume accounts for 10%, quartz powder accounts for 10%, quartz sand accounts for 25%, rubber particles account for 5%, and the water-cement ratio is 0.22, that is, the mass of water is 22% of the total mass of cement, silica fume and quartz powder, and the water reducer accounts for 1% of the mass of cement.
[0042] After step S3, gradually add water, water reducing agent and plasticizer to the dry mixture, stir at low speed for 3 minutes to allow water and powder to fully contact, and then stir at high speed for 5 minutes to ensure uniform mixing and no dry powder lumps.
[0043] The plasticizer is 0.5% of the cement mass.
[0044] After step S5, the mixed concrete is placed in a vacuum device for vacuum degassing to remove bubbles in the concrete for 10-15 minutes.
[0045] After vacuum degassing, use ultrasonic equipment to treat the concrete for 5-10 minutes. Ultrasonic energy can improve the uniformity and density of concrete and improve material properties.
[0046] After step S7, the mold is placed in a vacuum environment after pouring to further remove bubbles in the concrete and improve density and strength. The vacuum treatment time is 10-15 minutes.
[0047] After ultrasonic treatment, add 0.5% to 2% of the total mass of nanomaterials, including nano-silicon dioxide, and stir at a low speed for 2-5 minutes and at a high speed for 3-8 minutes.
[0048] After step S7, the concrete is cured using microwave equipment after casting to accelerate the initial and final setting of the concrete for 15-20 minutes.
[0049] Embodiment 2:
[0050] Please refer to the attached Figure 1 The present invention provides a method for preparing ultra-high performance rubber concrete, comprising the following specific steps:
[0051] S1: Material preparation, select silicate cement, microsilica powder, quartz powder, quartz sand, rubber particles, water and water reducing agent as raw materials for subsequent operations;
[0052] S2: Material weighing: use an electronic scale to weigh each raw material separately, and use a separate container to hold each material;
[0053] S3: Dry mixing: put high-grade cement, silica fume and quartz powder into a mixer according to the proportion, stir at low speed for 2 minutes to ensure preliminary mixing, then stir at high speed for 3 minutes to make the mixture uniform, add quartz sand, stir at low speed for 2 minutes, and stir at high speed for 3 minutes to ensure uniform distribution of each component;
[0054] S4: Add rubber particles. During the mixing process, gradually add the rubber particles and stir at a low speed for 2 minutes to disperse the rubber particles in the mixture, and then stir at a high speed for 5 minutes to ensure that the rubber particles are evenly distributed in the concrete;
[0055] S5: Wet mixing, continue mixing until the concrete is uniform and there are no dry powder lumps. The total mixing time is controlled within 5-10 minutes. Use a scraper or other tools to regularly scrape the mixture on the mixer wall to ensure that all materials are evenly mixed;
[0056] S6: Surface treatment of rubber particles. In order to improve the bonding performance between rubber particles and cement substrate, the rubber particles can be surface treated, for example, using silane coupling agent to treat the rubber particles, or roughening the surface of the rubber particles. Put the rubber particles in a container, add an appropriate amount of silane coupling agent solution - a 1:10 dilution of coupling agent and water, soak for 30 minutes, take out the rubber particles, dry them and set aside;
[0057] S7: Casting and molding. Pour the evenly mixed concrete into the mold, vibrate the mold with a vibrator to expel bubbles and improve the density of the concrete. The vibration time is controlled within 1-2 minutes. During the vibration process, observe whether there are bubbles escaping from the mold surface to ensure that there are no large bubbles inside the concrete.
[0058] S8: Curing. After pouring, standard curing is carried out at 20°C and relative humidity above 90% for 28 days to achieve the designed strength. Keep it moist during the curing period, cover it with wet burlap or spray it with curing liquid. Check the moisture content of the concrete regularly to avoid cracking of the concrete surface due to water loss.
[0059] The silicate cement in step S1 is selected as 52.5 grade silicate cement, the particle size of microsilica powder is 0.1-1 micron, the particle size of quartz powder is 10-100 micron, the particle size of quartz sand is 0.1-2 mm, and the particle size of rubber particles is 0.5-2 mm. In step S2, high-grade cement accounts for 45%, silica fume accounts for 7.5%, quartz powder accounts for 12.5%, quartz sand accounts for 25%, rubber particles account for 10%, and the water-cement ratio is 0.24, that is, the mass of water is 24% of the total mass of cement, silica fume and quartz powder, and the water reducer accounts for 1% of the mass of cement.
[0060] After step S3, gradually add water, water reducing agent and plasticizer to the dry mixture, stir at low speed for 3 minutes to allow water and powder to fully contact, and then stir at high speed for 5 minutes to ensure uniform mixing and no dry powder lumps.
[0061] The plasticizer is 0.5% of the cement mass.
[0062] After step S3, gradually add polypropylene fibers to the wet mixture, stir at a low speed for 2 minutes to ensure that the polypropylene fibers are evenly distributed, and then stir at a high speed for 3 minutes to fully mix the fibers into the concrete.
[0063] Polypropylene fiber accounts for 0.5%.
[0064] After step S5, the mixed concrete is placed in a vacuum device for vacuum degassing to remove bubbles in the concrete for 10-15 minutes.
[0065] After vacuum degassing, use ultrasonic equipment to treat the concrete for 5-10 minutes. Ultrasonic energy can improve the uniformity and density of concrete and improve material properties.
[0066] After step S7, the mold is placed in a vacuum environment after pouring to further remove bubbles in the concrete and improve density and strength. The vacuum treatment time is 10-15 minutes.
[0067] After ultrasonic treatment, add 0.5% to 2% of the total mass of nanomaterials, including nano-silicon dioxide, and stir at a low speed for 2-5 minutes and at a high speed for 3-8 minutes.
[0068] After step S7, the concrete is cured using microwave equipment after casting to accelerate the initial and final setting of the concrete for 15-20 minutes.
[0069] Embodiment three:
[0070] Please refer to the attached Figure 1 The present invention provides a method for preparing ultra-high performance rubber concrete, comprising the following specific steps:
[0071] S1: Material preparation, select silicate cement, microsilica powder, quartz powder, quartz sand, rubber particles, water and water reducing agent as raw materials for subsequent operations;
[0072] S2: Material weighing: use an electronic scale to weigh each raw material separately, and use a separate container to hold each material;
[0073] S3: Dry mixing: put high-grade cement, silica fume and quartz powder into a mixer according to the proportion, stir at low speed for 2 minutes to ensure preliminary mixing, then stir at high speed for 3 minutes to make the mixture uniform, add quartz sand, stir at low speed for 2 minutes, and stir at high speed for 3 minutes to ensure uniform distribution of each component;
[0074] S4: Add rubber particles. During the mixing process, gradually add the rubber particles and stir at a low speed for 2 minutes to disperse the rubber particles in the mixture, and then stir at a high speed for 5 minutes to ensure that the rubber particles are evenly distributed in the concrete;
[0075] S5: Wet mixing, continue mixing until the concrete is uniform and there are no dry powder lumps. The total mixing time is controlled within 5-10 minutes. Use a scraper or other tools to regularly scrape the mixture on the mixer wall to ensure that all materials are evenly mixed;
[0076] S6: Surface treatment of rubber particles. In order to improve the bonding performance between rubber particles and cement substrate, the rubber particles can be surface treated, for example, using silane coupling agent to treat the rubber particles, or roughening the surface of the rubber particles. Put the rubber particles in a container, add an appropriate amount of silane coupling agent solution - a 1:10 dilution of coupling agent and water, soak for 30 minutes, take out the rubber particles, dry them and set aside;
[0077] S7: Casting and molding. Pour the evenly mixed concrete into the mold, vibrate the mold with a vibrator to expel bubbles and improve the density of the concrete. The vibration time is controlled within 1-2 minutes. During the vibration process, observe whether there are bubbles escaping from the mold surface to ensure that there are no large bubbles inside the concrete.
[0078] S8: Curing. After pouring, standard curing is carried out at 20°C and relative humidity above 90% for 28 days to achieve the designed strength. Keep it moist during the curing period, cover it with wet burlap or spray it with curing liquid. Check the moisture content of the concrete regularly to avoid cracking of the concrete surface due to water loss.
[0079] In step S1, the silicate cement is selected as grade 52.5 silicate cement, the particle size of microsilica powder is 0.1-1 micron, the particle size of quartz powder is 10-100 micron, the particle size of quartz sand is 0.1-2 mm, and the particle size of rubber particles is 0.5-2 mm. In step S2, high-grade cement accounts for 55%, silica fume accounts for 5%, quartz powder accounts for 10%, quartz sand accounts for 20%, rubber particles account for 5%, and the water-cement ratio is 0.20, that is, the mass of water is 20% of the total mass of cement, silica fume and quartz powder, and the water reducer accounts for 1.5% of the cement mass.
[0080] After step S3, gradually add water, water reducing agent and plasticizer to the dry mixture, stir at low speed for 3 minutes to allow water and powder to fully contact, and then stir at high speed for 5 minutes to ensure uniform mixing and no dry powder lumps.
[0081] The plasticizer is 0.5% of the cement mass.
[0082] After step S3, gradually add the steel fibers to the wet mixture, stir at a low speed for 2 minutes to ensure that the steel fibers are evenly distributed, and then stir at a high speed for 3 minutes to fully mix the fibers into the concrete.
[0083] Steel fiber accounts for 2%.
[0084] After step S5, the mixed concrete is placed in a vacuum device for vacuum degassing to remove bubbles in the concrete for 10-15 minutes.
[0085] After vacuum degassing, use ultrasonic equipment to treat the concrete for 5-10 minutes. Ultrasonic energy can improve the uniformity and density of concrete and improve material properties.
[0086] After step S7, the mold is placed in a vacuum environment after pouring to further remove bubbles in the concrete and improve density and strength. The vacuum treatment time is 10-15 minutes.
[0087] After ultrasonic treatment, add 0.5% to 2% of the total mass of nanomaterials, including nano-silicon dioxide, and stir at a low speed for 2-5 minutes and at a high speed for 3-8 minutes.
[0088] After step S7, the concrete is cured using microwave equipment after casting to accelerate the initial and final setting of the concrete for 15-20 minutes.
[0089] Table 1: Comparison of properties of rubber concrete in different embodiments
[0090]
[0091]
[0092] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing ultra-high performance rubber concrete, characterized in that: The specific steps include: S1: Material preparation, selecting silicate cement, microsilica powder, quartz powder, quartz sand, rubber particles, water and water reducing agent as raw materials; S2: Material weighing: use an electronic scale to weigh each raw material separately, and use a separate container to hold each material; S3: Dry mixing: put high-grade cement, silica fume and quartz powder into a mixer according to the proportion, stir at low speed for 2-5 minutes, then stir at high speed for 2-5 minutes, then add quartz sand, stir at low speed for 1-3 minutes, and stir at high speed for 2-4 minutes; S4: Add rubber particles. During the stirring process, gradually add rubber particles, stir at a low speed for 2-5 minutes, and then stir at a high speed for 4-8 minutes; S5: Wet mixing, continue mixing until the concrete is uniform and there are no dry powder lumps, the total mixing time is controlled within 5-10 minutes, and use a scraper to scrape the mixture on the mixer wall regularly; S6: Surface treatment of rubber particles: put the rubber particles into a container, add an appropriate amount of silane coupling agent solution, which is a 1:10 dilution of the coupling agent and water, soak for 20-40 minutes, take out the rubber particles, and dry them for later use; S7: Casting and molding: pour the evenly mixed concrete into the mold, vibrate the mold with a vibrator to expel bubbles, and control the vibration time to 1-4 minutes. During the vibration process, observe whether there are bubbles escaping from the mold surface; S8: Curing: standard curing is carried out after pouring is completed. Curing is carried out for 25-30 days at 20℃-25℃ and relative humidity of 90%-100%. Keep it moist during curing, cover it with wet linen or spray it with curing liquid.
2. The method for preparing ultra-high performance rubber concrete according to claim 1, characterized in that: The silicate cement in step S1 is selected to be 52.5 grade silicate cement, the particle size of microsilica powder is 0.1-1 micron, the particle size of quartz powder is 10-100 micron, the particle size of quartz sand is 0.1-2 mm, and the particle size of rubber particles is 0.5-2 mm. In step S2, high-grade cement accounts for 45%-55%, silica fume accounts for 5%-10%, quartz powder accounts for 10%-15%, quartz sand accounts for 25%-35%, rubber particles account for 5%-10%, and the water-cement ratio is 0.20-0.25, that is, the mass of water is 20%-25% of the total mass of cement, silica fume and quartz powder, and the water reducer accounts for 0.8%-1.5% of the mass of cement.
3. The method for preparing ultra-high performance rubber concrete according to claim 1, characterized in that: After the step S3, water, a water reducing agent and a plasticizer are gradually added to the dry mixture, and the mixture is first stirred at a low speed for 3-6 minutes to allow the water and the powder to fully contact, and then stirred at a high speed for 3-6 minutes.
4. The method for preparing ultra-high performance rubber concrete according to claim 3, characterized in that: The plasticizer is 0.5%-1% of the mass of cement.
5. The method for preparing ultra-high performance rubber concrete according to claim 1, characterized in that: After the step S3, gradually add the fibers into the wet mixture, stir at a low speed for 2-5 minutes, and then stir at a high speed for 3-6 minutes to completely mix the fibers into the concrete.
6. The method for preparing ultra-high performance rubber concrete according to claim 5, characterized in that: The fiber accounts for 0.5%-2%.
7. The method for preparing ultra-high performance rubber concrete according to claim 1, characterized in that: After the step S5, the mixed concrete is placed in a vacuum device for vacuum degassing to remove bubbles in the concrete for 10-15 minutes.
8. The method for preparing ultra-high performance rubber concrete according to claim 7, characterized in that: After the vacuum degassing, the concrete is treated with ultrasonic equipment for 5-10 minutes.
9. The method for preparing ultra-high performance rubber concrete according to claim 7, characterized in that: After ultrasonic treatment, add 0.5% to 2% of the total mass of nanomaterials, including nano-silicon dioxide, and stir at a low speed for 2-5 minutes and at a high speed for 3-8 minutes.
10. The method for preparing ultra-high performance rubber concrete according to claim 1, characterized in that: After the step S7, the concrete is cured using microwave equipment after casting to accelerate the initial and final setting of the concrete for 15-20 minutes.