High-wear-resistance conductive misfire concrete and preparation method thereof

By using solid waste materials and limestone gravel, refractory materials, wear-resistant materials, conductive materials and nanopolymer composite materials in ignition-free concrete, the spark problem of ignition-free concrete after frictional static electricity is solved, and the wear resistance is improved and conductivity, meets the needs of high wear resistance, conductive and non-ignition concrete, and is suitable for special projects.

CN118930183AActive Publication Date: 2024-11-12CHINA CONSTR WEST CONSTR SOUTHWEST CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411141180.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Existing non-ignition concrete is prone to sparks after frictional static electricity gathering, resulting in structural damage and shortened service life, and failing to improve its wear resistance and non-ignition performance at the same time.

Method used

Solid waste materials and limestone gravel are used as fire-free aggregates, combined with refractory materials, wear-resistant agents, conductive materials and nanopolymer composite materials, significantly improve wear resistance and conductivity, reduce static aggregation, and form high wear-resistant conductivity. No fire concrete.

Benefits of technology

It significantly improves the wear resistance and conductivity of fire-free concrete, reduces static electricity aggregation, meets fire and explosion-proof requirements, extends service life, and promotes the reuse of solid waste resources. It is suitable for special projects with fire-proof explosion-proof requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses conductive misfire concrete with high wear resistance. The conductive misfire concrete is prepared from the following components in parts by weight: 290-355 parts of cement, 28-33 parts of fly ash, 48-53 parts of mineral powder, 1045-1135 parts of misfire coarse aggregate, 710-770 parts of misfire fine aggregate, 10-15 parts of a refractory material, 3-5.5 parts of a wear-resistant agent, 2-5 parts of a conductive material, 1.5-2.8 parts of a nano-composite high-molecular polymer, 4.5-6.4 parts of an additive and 140-185 parts of water, according to the invention, the solid waste material and the limestone gravel are used as misfire aggregates, and through the synergistic effect of the refractory material, the wear-resistant agent, the conductive material and the nano polymer composite material, the wear resistance and the conductivity are remarkably improved, so that the electrostatic aggregation in application is reduced; the obtained misfire concrete is excellent in working performance and mechanical performance, does not generate sparks and sparks after being polished and impacted, meets the fire protection requirements of fire protection and explosion prevention, and is suitable for being popularized and used in special projects with the fire protection and explosion prevention requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete materials, and in particular relates to a non-fireable concrete and a preparation method thereof. Background Art

[0002] Ordinary concrete and common building materials may generate sparks when encountering collision, impact and friction. The main reasons are that the building materials are hard, the raw materials or impurities contain metal substances, the friction or impact is too strong, and the friction easily generates static electricity. If the building is a flammable and explosive place, such as an oil depot, a gas plant, etc., explosions, combustion and other accidents that seriously endanger life safety may occur.

[0003] Non-fireable concrete, also known as explosion-proof concrete, is an inorganic non-metallic material made by mixing silicate cement as a cementitious material, certain mixed materials and admixtures, non-fireable aggregates and water in a certain proportion. It does not produce sparks or sparks when it undergoes mechanical movements such as friction and impact with hard objects such as metals or stones, and does not cause the risk of ignition or explosion of flammable materials. It is a special concrete with non-fireable properties. However, due to the particularity of its requirements, it is not widely used in commercial concrete.

[0004] The invention patent "A non-fireable concrete and its preparation method" (CN 202311357041.1) utilizes solid waste resources to select dolomite waste rock to make sand and gravel as aggregate, and uses fly ash and phosphorus slag powder as admixtures. Solid waste resources are used extensively to obtain non-fireable concrete with excellent working performance and mechanical properties. The concrete does not produce sparks after metal grinding, impact, and chopping, which meets the call for comprehensive utilization of solid waste. However, the two influencing factors of friction static electricity and wear resistance are not considered as a whole. In the above-mentioned related technologies, non-fireable concrete often generates static electricity after friction defects during use, which causes sparks, causing damage to the concrete structure and greatly shortening the service life of the non-fireable concrete. Therefore, how to reduce the wear and static electricity accumulation of non-fireable concrete while increasing its non-fireable performance is a problem that needs to be solved urgently. Summary of the invention

[0005] In view of the above problems, the present invention provides a highly wear-resistant conductive non-fired concrete and a preparation method thereof, which uses solid waste materials and limestone crushed stone as non-fired aggregates, and significantly increases the wear resistance and conductivity through the synergistic effect of refractory materials, wear resistant agents, conductive materials and nano-polymer composite materials, thereby reducing the static electricity accumulation during application; the obtained non-fired concrete has excellent working performance and mechanical properties, and the concrete does not produce sparks after grinding and impact, meets the fire protection requirements of fire prevention and explosion prevention, and is suitable for promotion and use in special projects with fire protection and explosion prevention requirements.

[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0007] A highly wear-resistant conductive non-fireable concrete, the composition of which is as follows in parts by weight:

[0008] 290-355 parts of cement, 28-33 parts of fly ash, 48-53 parts of mineral powder, 1045-1135 parts of non-pyrophoric coarse aggregate, 710-770 parts of non-pyrophoric fine aggregate, 10-15 parts of refractory materials, 3-5.5 parts of wear resistant agents, 2-5 parts of conductive materials, 1.5-2.8 parts of nano-composite high molecular polymers, 4.5-6.4 parts of admixtures, and 140-185 parts of water.

[0009] According to the above scheme, the cement is ordinary Portland cement 42.5R; the fly ash is Class F II fly ash with a density of 2.2-2.4 g / cm 3 The ignition loss is 5.0-5.4%; the mineral powder is S95 mineral powder, and the density is 3.1-3.3g / cm 3 , the fluidity ratio is 95~97%.

[0010] According to the above scheme, the non-fired coarse aggregate is a mixture of limestone crushed stone and waste furnace lining, the mass ratio of limestone crushed stone to waste furnace lining is (6.5-8.5):3.5, the particle size is 5-16mm, and the overall crushing index is 13-15%; the waste furnace lining is waste alkaline refractory material of glass kiln, and the main components are calcium oxide and magnesium oxide.

[0011] The abandoned furnace lining is fire-resistant, resistant to mechanical impact and wear. While enhancing the wear resistance and non-inflammable properties of non-inflammable concrete, it reduces the use of limestone gravel, is environmentally friendly and energy-saving, reduces waste emissions, and increases resource utilization.

[0012] According to the above scheme, the non-pyrophoric fine aggregate is a mixture of limestone machine-made sand and waste solar panel particles, and the mass ratio of limestone machine-made sand to waste solar panel particles is (4-6):1; the limestone machine-made sand adopts a continuous grading below 4.75 mm, and the fineness modulus is 2.7-3.0; the waste solar panel particles are obtained by crushing waste solar panels, the main component is polysilicon, and the particle size is 0.15 mm-0.3 mm.

[0013] Due to their characteristics, waste solar panel particles have excellent electrical conductivity, which can significantly enhance the electrical conductivity of non-fireable concrete, reduce static electricity accumulation in non-fireable concrete, and reduce the probability of fire.

[0014] According to the above scheme, the refractory material is expanded vermiculite powder, which is yellow-brown in color and has a particle size of 200 to 300 meshes.

[0015] Expanded vermiculite powder has good thermal insulation properties and high temperature resistance, and can effectively reduce the flammability of concrete at high temperatures.

[0016] According to the above scheme, the wear-resistant agent is a mixture of vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume, and the mass ratio of vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume is (2.1-3.5):(4.2-5.6):1; the silica fume is densified silica fume, with a silicon dioxide content of 92%-94% and a bulk density of 450kg / m 3 ~500kg / m 3 .

[0017] Vinyl acetate-ethylene copolymer emulsion and polyacrylate are both used to improve the bonding strength between cement-based materials and aggregates, thereby improving the wear resistance of concrete. Silica fume has a small fineness and is used to fill the gaps between cement-based materials and aggregates, thereby enhancing the compactness and surface hardness of concrete and improving the wear resistance of concrete.

[0018] According to the above scheme, the conductive material is a mixture of carbonized rice husk powder and carbon fiber, and the mass ratio of carbonized rice husk powder to carbon fiber is 1:1; wherein the fineness of the carbonized rice husk powder is 100-200 mesh; and the size of the carbon fiber is 1-2 cm.

[0019] According to the above scheme, the preparation method of the nanocomposite high molecular polymer comprises the following steps:

[0020] (1) Graphite powder, sodium dodecylbenzene sulfonate, sodium hydroxide, and a portion of deionized water are stirred and mixed uniformly, and then hydroxymethyl cellulose is added and stirred continuously and ultrasonically dispersed to obtain a suspension.

[0021] (2) dispersing the sodium montmorillonite and ammonium polyphosphate in the remaining deionized water with high-speed stirring and dispersion, and mixing with the suspension obtained in step 1 with high-speed stirring and dispersion after stagnating;

[0022] (3) placing the mixture in a closed container, heating it to 80° C. and stirring it for 5 h, and cooling it to obtain a nanocomposite polymer;

[0023] The raw materials used are calculated by weight as follows: 5-8 parts of graphite powder, 20-33 parts of hydroxymethyl cellulose, 44-58 parts of sodium montmorillonite, 0.5-1.0 parts of sodium dodecylbenzene sulfonate, 1.1-1.5 parts of sodium hydroxide, 2.2-3.2 parts of ammonium polyphosphate, and 125-155 parts of deionized water; the fineness of the graphite powder is 5-10 μm; the fineness of the sodium montmorillonite is 100-300 nm.

[0024] The graphite powder provides a conductive effect, and sodium dodecylbenzene sulfonate serves as a surfactant to disperse the suspension while also guiding and eliminating the accumulation of harmful charges; hydroxymethyl cellulose improves the internal connectivity of concrete and the mechanical properties of concrete, and on the other hand, after being flame-retardantly modified, it is dehydrated and carbonized in advance to form a dense carbon layer, which inhibits its further decomposition and improves the flame retardancy and conductivity of the matrix material; sodium-based montmorillonite plays a flame-retardant role, and has significant wear resistance after being compounded with cellulose and graphite; sodium hydroxide plays a role in promoting the dissolution of hydroxymethyl cellulose; ammonium polyphosphate plays an auxiliary synergistic combustion-supporting role, and reacts with the hydroxyl group on the pyranose ring of cellulose to generate cell-dense carbon, thereby limiting the transfer of heat and improving the thermal stability of concrete; through the synergy of various components, a nano-composite high molecular polymer with wear resistance, flame retardancy and conductivity is generated.

[0025] According to the above scheme, the admixture is a polycarboxylic acid high-efficiency water reducing agent with a solid content of 12wt% and a water reduction rate of 26%.

[0026] The method for preparing the above-mentioned highly wear-resistant conductive non-fireable concrete comprises the following steps:

[0027] (1) Premix the non-pyrophoric coarse aggregate, non-pyrophoric fine aggregate, wear-resistant agent and one-third of water in a mixer for 1 minute;

[0028] (2) Cement, fly ash, mineral powder, refractory material, conductive material, admixture, remaining two-thirds of water and nano-composite high molecular polymer are then added into a mixer and stirred for 3 minutes; after being stirred and mixed evenly, the mixture is poured out to obtain a finished product of highly wear-resistant conductive non-fireable concrete.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] In addition to limestone crushed stone, the non-fired coarse and fine aggregates of the present invention are also mixed with waste glass kiln linings and waste solar panel particles. The two materials do not ignite due to friction due to their materials. The use of the two materials can significantly reduce the amount of limestone aggregate, thereby reducing production costs, and the mixed use of aggregates of different materials can also reduce the concrete performance problems under a single type of aggregate; secondly, the two materials are construction solid waste resources, and the application of them in non-fired concrete can promote their recycling rate, reduce their impact on the environment, save energy, protect the environment, and be green and low-carbon; finally, the waste slag has excellent wear resistance, and the waste solar panel particles have excellent electrical conductivity. The application of them in non-fired concrete in coordination with wear-resistant agents and conductive materials can significantly improve their wear resistance and electrical conductivity.

[0031] The wear-resistant agent of the present invention uses a mixture of vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume. The mechanism of vinyl acetate-ethylene copolymer emulsion and polyacrylate is to form a network structure in concrete, so that the bonding force between cement-based materials and aggregates is stronger, thereby improving the wear resistance of concrete, and the mechanism of silica fume is to fill the gap between cement-based materials and aggregates to enhance the strength, density and surface hardness of concrete, thereby improving the wear resistance of concrete. The beneficial effects of the three can be superimposed to further improve the wear resistance of concrete.

[0032] The nano composite high molecular polymer of the present invention is a graphite / cellulose / clay nano composite polymer. Graphite and cellulose are added to montmorillonite. Through a simple heating reaction, the montmorillonite and graphite are uniformly dispersed in a polymer matrix to form a "delaminated nano composite material". Then, through the synergistic effect of sodium dodecylbenzene sulfonate, ammonium polyphosphate and the like, a high-performance nano composite high molecular polymer with wear resistance, flame retardancy and electrical conductivity is generated. The nano composite high molecular polymer is applied to non-fired concrete to significantly improve the wear resistance, electrical conductivity and flame retardancy of the non-fired concrete and reduce its ignition probability.

[0033] The present invention not only increases the incombustibility of incombustible concrete, but also incorporates refractory materials and montmorillonite components, which play a role in heat insulation and preventing the escape of combustible gas during thermal decomposition and combustion, and can effectively reduce the combustibility of incombustible concrete at high temperatures. The present invention aims to improve the incombustibility of incombustible concrete while reducing its combustion reaction after ignition, ensure the service performance of construction, and provide performance guarantee for construction in special occasions. DETAILED DESCRIPTION

[0034] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0035] The specific embodiment provides a method for preparing a nanocomposite polymer:

[0036] (1) Graphite powder, sodium dodecylbenzene sulfonate, sodium hydroxide and a portion of deionized water are placed in a beaker and stirred under a magnetic stirrer for 1 hour, then hydroxymethyl cellulose is added and stirred for 2 hours, then the beaker is taken out and placed under an ultrasonic disperser for ultrasonic dispersion for 1 hour to obtain a suspension;

[0037] (2) dispersing sodium montmorillonite and ammonium polyphosphate in the remaining deionized water, and using a digital high-speed disperser to operate at a speed of 8000 rpm for 1.5 hours; after stagnating, adding the suspension stirred in step (1), and continuing to operate at a speed of 8000 rpm for 2 hours to obtain a uniformly mixed mixture;

[0038] (3) Finally, the mixed solution was poured into a beaker, the beaker mouth was sealed, and the mixture was placed on a magnetic stirrer and stirred at 80° C. for 5 h. After cooling, a nanocomposite polymer was obtained.

[0039] The specific embodiment also provides a method for preparing highly wear-resistant conductive non-fireable concrete:

[0040] (1) Add the weighed incombustible coarse aggregate, incombustible fine aggregate, wear-resistant agent and one-third of water into a clean mixer and premix for 1 minute;

[0041] (2) Cement, fly ash, mineral powder, refractory material, conductive material, admixture, remaining two-thirds of water and nano-composite high molecular polymer are then added into a mixer and stirred for 3 minutes; after being stirred and mixed evenly, the mixture is poured out to obtain a finished product of highly wear-resistant conductive non-fireable concrete.

[0042] In the following examples, the cement used is ordinary Portland cement 42.5R; the fly ash used is Class F II fly ash with a density of 2.4 g / cm 3 The ignition loss is 5.4%; the ore powder uses S95 ore powder with a density of 3.1g / cm 3 , fluidity ratio 97%; limestone crushed stone adopts particle size 5-16mm, and the overall crushing index is 13-15%; waste furnace lining adopts waste alkaline refractory material of glass kiln, with particle size 5-16mm and overall crushing index 13-15%; limestone machine-made sand adopts continuous graded machine sand below 4.75mm, and fineness modulus 2.7-3.0; the main component of waste solar panel particles is polysilicon, with particle size of 0.15mm-0.3mm; expanded vermiculite powder is yellow-brown in color, with particle size of 200-300 mesh; carbonized rice husk powder is obtained by grinding carbonized rice husk, and the carbonized rice husk is purchased through conventional commercial channels with a size of 2-4cm, and then ground by ball mill to obtain carbonized rice husk powder with a fineness of 100-200 mesh; carbon fiber size is 1-2cm.

[0043] Example 1

[0044] A highly wear-resistant conductive non-fireable concrete, the composition of which is as follows:

[0045] 300 parts of cement, 28 parts of fly ash, 48 parts of mineral powder, 1055 parts of non-fired coarse aggregate, 725 parts of non-fired fine aggregate, 10 parts of refractory material, 3.2 parts of wear resistant agent, 2.8 parts of conductive material, 1.8 parts of nano-composite high molecular polymer, and 150 parts of water.

[0046] Among them, the mass ratio of limestone crushed stone to waste furnace lining in non-fired coarse aggregate is 6.5:3.5; the mass ratio of limestone machine-made sand to waste solar panel particles in non-fired fine aggregate is 4:1; the mass ratio of wear-resistant agents vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume is 2.5:4.4:1; the mass ratio of conductive material carbonized rice husk powder to carbon fiber is 1:1.

[0047] The nano-composite high molecular polymer includes 5 parts of graphite powder, 22 parts of hydroxymethyl cellulose, 48 parts of sodium montmorillonite, 0.6 parts of sodium dodecylbenzene sulfonate, 1.2 parts of sodium hydroxide, 2.5 parts of ammonium polyphosphate and 130 parts of deionized water.

[0048] Example 2

[0049] 320 parts of cement, 30 parts of fly ash, 51 parts of mineral powder, 1070 parts of non-pyrophoric coarse aggregate, 750 parts of non-pyrophoric fine aggregate, 12 parts of refractory material, 4.1 parts of wear resistant agent, 3.5 parts of conductive material, 2.0 parts of nano-composite high molecular polymer, and 160 parts of water.

[0050] Among them, the mass ratio of limestone crushed stone to waste furnace lining in non-fired coarse aggregate is 7:3.5; the mass ratio of limestone machine-made sand to waste solar panel particles in non-fired fine aggregate is 5:1; the mass ratio of wear-resistant agents vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume is 3:4.8:1; the mass ratio of conductive material carbonized rice husk powder to carbon fiber is 1:1.

[0051] The nano-composite high molecular polymer includes 6.5 parts of graphite powder, 26 parts of hydroxymethyl cellulose, 52 parts of sodium montmorillonite, 0.8 parts of sodium dodecylbenzene sulfonate, 1.2 parts of sodium hydroxide, 2.7 parts of ammonium polyphosphate and 142 parts of deionized water.

[0052] Example 3

[0053] 350 parts of cement, 32 parts of fly ash, 52 parts of mineral powder, 1110 parts of non-pyrophoric coarse aggregate, 770 parts of non-pyrophoric fine aggregate, 15 parts of refractory materials, 5 parts of wear resistant agents, 4.5 parts of conductive materials, 2.5 parts of nano-composite high molecular polymers, 2.6 parts of admixtures, and 170 parts of water.

[0054] Among them, the mass ratio of limestone crushed stone to waste furnace lining in non-fired coarse aggregate is 8.1:3.5; the mass ratio of limestone machine-made sand to waste solar panel particles in non-fired fine aggregate is 6:1; the mass ratio of wear-resistant agents vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume is 3.2:5.4:1; the mass ratio of conductive material carbonized rice husk powder to carbon fiber is 1:1.

[0055] The nano-composite high molecular polymer includes 7.7 parts of graphite powder, 32 parts of hydroxymethyl cellulose, 56 parts of sodium montmorillonite, 1.0 parts of sodium dodecylbenzene sulfonate, 1.4 parts of sodium hydroxide, 3.0 parts of ammonium polyphosphate and 150 parts of deionized water.

[0056] Basic comparison

[0057] Based on Example 2, waste furnace lining, waste solar panel particles, refractory materials, wear resistant agents, conductive materials and nano-composite polymers are not added, and other components and preparation processes remain unchanged.

[0058] Comparative Example 1

[0059] Based on Example 2, the coarse aggregate and the fine aggregate were replaced with limestone aggregate alone, and the other components and preparation process remained unchanged.

[0060] Comparative Example 2

[0061] Based on Example 2, the refractory expanded vermiculite powder is not added, and the other components and preparation process remain unchanged.

[0062] Comparative Example 3

[0063] Based on Example 2, no anti-wear agent component is added, and other components and preparation process remain unchanged.

[0064] Comparative Example 4

[0065] Based on Example 2, no conductive material component is added, and other components and preparation process remain unchanged.

[0066] Comparative Example 5

[0067] Based on Example 2, no nanocomposite high molecular polymer component is added, and other components and preparation process remain unchanged.

[0068] The various properties of the non-fired concrete of the above-mentioned Examples 1-3, the basic comparative example and the comparative examples 1-5 were tested, including compressive strength, non-fire performance, wear resistance, fire resistance and electrical conductivity, and the results are shown in Table 1. The compressive strength of each group of non-fired concrete meets the standard.

[0069] Non-inflammability: The diameter of the grinding wheel used in the test is 150mm, and its rotation speed during the test is 1000r / min. Its ability to separate sparks is checked in a dark room. When each specimen is rubbed on the grinding wheel, a pressure of 20N is applied. After any part of the specimen is brought into contact with the grinding wheel, carefully observe the friction between the concrete specimen and the grinding wheel to see if there is any spark.

[0070] Wear resistance: The wear resistance of concrete was tested in accordance with the national standard GB T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". The size of the concrete specimen was 150mm×150mm×150mm, and the wear resistance was characterized by the amount of wear.

[0071] Fire resistance: The fire resistance of concrete is tested in accordance with the national standard GB / T 7322-2017 "Test method for fire resistance of refractory materials". The test piece is prepared as a truncated triangular cone. The fire resistance temperature when it is heated at a specified rate until the tip of the cone bends and contacts the base is taken as the refractoriness, which is used to characterize the fire resistance of concrete.

[0072] Conductive properties: Use a concrete resistivity tester to measure the resistivity of the concrete standard test block.

[0073] Table 1 Test performance parameters of non-fired concrete

[0074] category No ignition performance <![CDATA[Wear amount (g / m 2 )]]> Refractoriness(℃) Resistivity (Ω·cm) Example 1 Don't get angry 2.56 262 4.3 Example 2 Don't get angry 1.65 346 3.0 Example 3 Don't get angry 2.16 304 3.8 Basic comparison Don't get angry 3.74 143 7.8 Comparative Example 1 Don't get angry 2.35 322 3.5 Comparative Example 2 Don't get angry 1.71 228 3.2 Comparative Example 3 Don't get angry 3.08 335 3.3 Comparative Example 4 Don't get angry 1.67 329 6.3 Comparative Example 5 Don't get angry 2.03 197 4.8

[0075] It can be seen from Table 1 that the non-fire performance of each group of non-fire concrete meets the standard, and the various parameters of the non-fire concrete of Examples 1-3 and Comparative Examples 1-5 are better than those of the basic comparative example, which shows that the addition of various components significantly improves the performance of the non-fire concrete, optimizes the use performance of the non-fire concrete, and reduces the non-fire performance of the concrete.

[0076] Comparing Examples 1-3, it can be seen that the various properties of the non-fired concrete show a trend of first increasing and then decreasing with the increase of the dosage of each external component, but it is still better than the basic comparative example; this shows that when the dosage of the external component is small, the various properties of the non-fired concrete are gradually improved; when the dosage reaches a certain point, if it continues to be added, the performance of the non-fired concrete will gradually decrease. On the one hand, the reason is that after the dosage is too high, the mechanical properties and density of the concrete itself are reduced, which in turn causes an increase in abrasion, a decrease in refractoriness, and an increase in resistivity; on the other hand, the reason is that after the external component is increased, it cannot be evenly dispersed inside the concrete, which not only cannot improve the performance of the concrete, but even has a negative impact on it. Therefore, when adding external components to the non-fired concrete, it is necessary to pay attention to the dosage problem. Overall, the non-fired concrete of Example 2 has excellent performance and can be widely used in special projects with fire protection and explosion-proof requirements.

[0077] Comparing Example 2 with Comparative Examples 1-5, when the composite aggregate is replaced with a single limestone aggregate, the abrasion of the non-fired concrete increases, the refractoriness decreases, and the resistivity increases, among which the abrasion has the greatest impact, followed by the resistivity, and finally the refractoriness, indicating that the waste slag and waste solar panel particles can significantly improve the performance of the non-fired concrete; when the refractory material expanded vermiculite powder is not added, the refractoriness of the non-fired concrete decreases significantly, but the other two properties are basically unchanged, indicating that the expanded vermiculite powder only plays a single flame retardant role and has basically no effect on other properties; when the wear-resistant agent is not added, the abrasion of the non-fired concrete is significantly When the conductive material is not added, the resistivity of the non-fired concrete increases significantly, but the other two properties remain basically unchanged, indicating that the wear-resistant agent only plays a single wear-resistant role and has little effect on other properties; when the conductive material is not added, the resistivity of the non-fired concrete increases significantly, but the other two properties remain basically unchanged, indicating that the conductive material only plays a single conductive role and has little effect on other properties; when the nano-composite polymer is not added, the abrasion of the non-fired concrete increases, the refractoriness decreases, and the resistivity increases, among which the refractoriness has the greatest impact, followed by the resistivity, and finally the abrasion, indicating that the nano-composite polymer can significantly improve the performance of the non-fired concrete.

[0078] The general causes of ignition include two aspects: mechanical impact and friction that produces static electricity. When the spark reaches a certain energy and the external conditions are met, it will cause a disaster of combustion and explosion, so concrete must be non-flammable to ensure safety. Conductive materials are conducive to the rapid transfer of charges, can quickly conduct away unfavorable charges, avoid the concentration of charges to produce sparks, and thus improve the non-flammable performance of concrete; wear-resistant agents can reduce unnecessary friction losses and reduce the possibility of sparks; refractory materials can improve the refractoriness of concrete and can effectively reduce the flammability of non-flammable concrete at high temperatures; composite aggregates can effectively improve the working performance of concrete, and together with nano-composite polymers can improve the wear resistance and refractoriness of concrete, reduce its conductivity, and improve the non-flammable performance of concrete as a whole. In summary, composite aggregates, refractory materials, wear-resistant agents, conductive materials and nano-composite polymers can enhance the non-flammable performance of non-flammable concrete from a single or multiple perspectives, and the synergy of each component can improve the non-flammable performance of non-flammable concrete as a whole.

[0079] The highly wear-resistant conductive non-fireable concrete prepared by the present invention has excellent non-fireable and wear-resistant properties and good application value. On the other hand, solid waste is used, which plays a positive role in the recovery and reuse of industrial solid materials and has a significant effect on energy conservation, emission reduction and green and sustainable development in the construction industry.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly wear-resistant conductive non-fireable concrete, characterized in that The composition is calculated by weight as follows: 290-355 parts of cement, 28-33 parts of fly ash, 48-53 parts of mineral powder, 1045-1135 parts of non-pyrophoric coarse aggregate, 710-770 parts of non-pyrophoric fine aggregate, 10-15 parts of refractory materials, 3-5.5 parts of wear resistant agents, 2-5 parts of conductive materials, 1.5-2.8 parts of nano-composite high molecular polymers, 4.5-6.4 parts of admixtures, and 140-185 parts of water.

2. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The cement is ordinary Portland cement 42.5R; the fly ash is Class F II fly ash with a density of 2.2-2.4 g / cm 3 The ignition loss is 5.0-5.4%; the mineral powder is S95 mineral powder, and the density is 3.1-3.3g / cm 3 , the fluidity ratio is 95~97%.

3. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The non-fired coarse aggregate is a mixture of limestone crushed stone and waste furnace lining, the mass ratio of limestone crushed stone to waste furnace lining is (6.5-8.5):3.5, the particle size is 5-16 mm, and the overall crushing index is 13-15%; the waste furnace lining is waste alkaline refractory material of glass kiln, and the main components are calcium oxide and magnesium oxide.

4. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The non-pyrophoric fine aggregate is a mixture of limestone machine-made sand and waste solar panel particles, and the mass ratio of limestone machine-made sand to waste solar panel particles is (4-6):1; the limestone machine-made sand adopts a continuous grading below 4.75 mm, and a fineness modulus of 2.7-3.0; the waste solar panel particles are obtained by crushing waste solar panels, the main component of which is polysilicon, and the particle size is 0.15 mm-0.3 mm.

5. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The refractory material is expanded vermiculite powder, which is yellow-brown in color and has a particle size of 200 to 300 meshes.

6. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The wear-resistant agent is a mixture of vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume, and the mass ratio of vinyl acetate-ethylene copolymer emulsion, polyacrylate and silica fume is (2.1-3.5):(4.2-5.6):1; the silica fume is densified silica fume, the silicon dioxide content is 92%-94%, and the bulk density is 450kg / m 3 ~500kg / m 3 .

7. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The conductive material is a mixture of carbonized rice husk powder and carbon fiber, and the mass ratio of the carbonized rice husk powder to the carbon fiber is 1:1; wherein the fineness of the carbonized rice husk powder is 100-200 meshes; and the size of the carbon fiber is 1-2 cm.

8. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The preparation method of the nanocomposite high molecular polymer comprises the following steps: (1) Graphite powder, sodium dodecylbenzene sulfonate, sodium hydroxide, and a portion of deionized water are stirred and mixed uniformly, and then hydroxymethyl cellulose is added and stirred continuously and ultrasonically dispersed to obtain a suspension. (2) dispersing the sodium montmorillonite and ammonium polyphosphate in the remaining deionized water with high-speed stirring and dispersion, and mixing with the suspension obtained in step 1 with high-speed stirring and dispersion after stagnating; (3) placing the mixture in a closed container, heating it to 80° C. and stirring it for 5 h, and cooling it to obtain a nanocomposite polymer; The raw materials used are calculated by weight as follows: 5-8 parts of graphite powder, 20-33 parts of hydroxymethyl cellulose, 44-58 parts of sodium montmorillonite, 0.5-1.0 parts of sodium dodecylbenzene sulfonate, 1.1-1.5 parts of sodium hydroxide, 2.2-3.2 parts of ammonium polyphosphate, and 125-155 parts of deionized water; the fineness of the graphite powder is 5-10 μm; the fineness of the sodium montmorillonite is 100-300 nm.

9. The highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The admixture is a polycarboxylic acid high-efficiency water reducing agent with a solid content of 12wt% and a water reducing rate of 26%.

10. The method for preparing the highly wear-resistant conductive non-refractory concrete according to claim 1, characterized in that The steps include: (1) Premix the non-pyrophoric coarse aggregate, non-pyrophoric fine aggregate, wear-resistant agent and one-third of water in a mixer for 1 minute; (2) Cement, fly ash, mineral powder, refractory material, conductive material, admixture, remaining two-thirds of water and nano-composite high molecular polymer are then added into a mixer and stirred for 3 minutes; after being stirred and mixed evenly, the mixture is poured out to obtain a finished product of highly wear-resistant conductive non-fireable concrete.

Citation Information

Patent Citations

  • Non-sparking wear-resisting concrete and method for carrying out floor construction through concrete

    CN106587823A

  • Non-sparking concrete and preparation method therefor

    CN106747013A

  • Non-sparking concrete and preparation method thereof

    CN112079606A

  • Impermeable anti-dry-shrinkage highly-homogeneous self-compacting concrete and preparation process thereof

    CN113024166A

  • Heat-resistant concrete and production process thereof

    CN113443868A