Preparation method of six-membered layered high-entropy MAX phase ceramic

By using pure metal or metal carbide powder and graphite powder, combined with ball milling, drying and sintering processes, the six-member high-entropy MAX phase ceramic material was successfully prepared, solving the problems of high costs and impurities in the existing technology, and achieving high quality Performance and low cost high entropy MAX phase material synthesis, especially in tribological properties.

CN118930270AActive Publication Date: 2024-11-12LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411219109.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The existing 413 high-entropy MAX phase material synthesis technology has problems with high cost and impurities, making it difficult to achieve high-purity phase and low-cost synthesis.

Method used

Using pure metal powder or metal carbide powder and graphite powder as raw materials, six-member layered high-entropy MAX phase ceramic material (Ti0.25V0.25Nb0) is prepared by ball milling, drying, cold press forming and discharge plasma or hot press sintering processes. .25Ta0.25)4AlC3 avoids the use of high-cost 211 single-element MAX phase and catalyst-like catalysts.

Benefits of technology

The high-entropy MAX phase material synthesis with low cost and simple process is realized. The obtained materials have better tribological properties than the high-entropy MAX phase of the same element, and are free of impurity pollution, and have better tribological properties in wide temperature domain.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930270A_ABST
    Figure CN118930270A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of six-membered layered high-entropy MAX phase (Ti0. 25V0. 25Nb0. 25Ta0. 25) 4AlC3 ceramic, which comprises the following steps: mixing four kinds of M-site metal powder, Al powder and C powder in proportion as raw materials, or carrying out sintering reaction by taking two kinds of carbide powder of NbC and TaC and residual element pure metal powder as raw materials to prepare a 413 type layered high-entropy MAX phase material. The preparation method comprises the following steps: by taking alcohol as a grinding medium, carrying out ball milling on raw materials in an argon environment for 10-12 hours to obtain mixed powder, drying the mixed powder in a vacuum environment at 60 DEG C for 10-24 hours, carrying out cold pressing on the dried mixed powder to obtain a blank, and then carrying out spark plasma sintering or hot pressed sintering to obtain the target layered high-entropy MAX phase material. Through inspection, compared with the same-element 211 type (Ti0. 25V0. 25Nb0. 25Ta0. 25) 2AlC MAX phase ceramic, the 413 type high-entropy ceramic material has more excellent tribological performance in a wide temperature range, and has a larger potential application prospect under extremely complex working conditions such as high temperature and high load. The preparation method is simple in process, low in raw material cost and easy for industrial large-scale production, and lays a foundation for application of the high-entropy MAX phase material in the friction field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of layered high-entropy ceramic materials, and in particular relates to a six-element high-entropy MAX phase ceramic material and a preparation method thereof. Background Art

[0002] MAX phase is a type of carbide, nitride or carbonitride with a layered microstructure. Its molecular formula is M n+1 AX n , n=1, 2, 3 or 4, M is a pre-transition element, A is mainly a third, fourth or fifth main group element, and X is C or N. There is an ionic bond or a covalent bond between M and X, and a metallic bond between M and A. Therefore, the MAX phase can have the advantages of both ceramics and metals, such as low density, high modulus, high damage tolerance and good machinability.

[0003] The concept of "high entropy" was originally developed from high entropy alloys. Ye Weijun proposed the concept of high entropy alloys in 2004, that is, multiple alloy elements are dissolved together in nearly equal molar ratios to form a single-phase solid solution. High entropy ceramics inherit the design concept of high entropy alloys and are single-phase ceramics composed of no less than four types of cations or anions. The "high entropy effect" caused by multiple principal elements improves the thermal stability of ceramic materials, and the solid solution strengthening and lattice distortion caused by "high entropy" can further improve the mechanical properties of the material. The "cocktail" effect can make the performance of high entropy materials better than that of ceramic materials of each single element.

[0004] High-entropy MAX phase ceramics are a new type of MAX phase material that has emerged in recent years. They have higher hardness, strength and thermal stability than traditional MAX phase ceramics. The designability of high-entropy multi-main elements can give them unique physical and chemical properties, and they have broad application prospects in the fields of aerospace and nuclear power structural materials, magnetism and thermoelectricity. In addition, the unique layered microstructure of the MAX phase gives it a lot of exploration space and good application prospects in the field of friction and wear. At present, there are few studies on the synthesis of high-entropy 413-type MAX phase materials (Journal of the European Ceramic Society, 2021, 41(8): 4658-4665). The synthesis of the 413-type MAX phase reported in the report uses single-element 211-type MAX powder, and requires the presence of a catalyst-like phase for synthesis, which not only increases the difficulty of synthesis, but also increases the cost of synthesis. In addition, the catalyst-like phase will eventually exist in the target product in the form of an intermetallic compound, making it impossible for the target product to reach a high-purity phase. Therefore, using low-cost pure metal powder or carbide powder and simple process to synthesize new high-entropy MAX phase materials is an inevitable choice to broaden the types of high-entropy MAX phase materials and expand their applications in the field of tribology. Summary of the invention

[0005] The present invention aims to solve the current technical problems regarding the synthesis of 413 type high entropy MAX phases to a certain extent. To this end, the main purpose of the present invention is to provide a method for preparing a six-element layered high entropy MAX phase ceramic, the molecular formula of which is (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The characteristic is that the raw materials used for synthesis do not require the high-cost 211 type single-element MAX phase. Metal elements, metal carbides, aluminum powder and graphite powder are used as raw materials. The 413 type high-entropy MAX phase ceramic material synthesized according to the present invention has better tribological properties than the same element 211 type high-entropy MAX phase material, and the synthesis cost is low and the process is simple.

[0006] The technical solution provided by the present invention is as follows: A method for preparing a six-element layered high entropy MAX phase ceramic, the preparation steps are as follows: (1) M-site metal element powder, Al powder and C powder are mixed in proportion as raw materials, and the M-site metal powder includes Ti powder, V powder, Nb powder and Ta powder; or NbC and TaC carbide powder are used instead of Nb powder and Ta powder, and then mixed with Ti powder, V powder and Al powder in proportion as raw materials.

[0007] Wherein, M-site Ti powder, V powder, Nb powder and Ta powder are mixed in equal molar ratios, the molar ratio of M-site metal powder: Al powder: C powder is 2: (1.1-1.2): 0.9; the molar ratio of Ti powder: V powder: NbC powder: TaC powder: Al powder is 0.5: 0.5: 0.5: 0.5: (1.1-1.2); The purity of the above raw materials Ti powder, V powder, Nb powder, Ta powder, NbC powder, TaC powder, Al powder and C powder is ≥99%, and the powder particle size is not less than 325 mesh.

[0008] (2) The raw materials in step 1) are ball-milled for 10 to 12 hours under an argon protection environment, and 30% to 40% of the total weight of anhydrous ethanol is added as a ball-milling medium, and a mixed powder is obtained after grinding; the ball-to-material ratio of the ball mill is (2 to 3): 1, and the ball milling speed is 200 to 400 rpm.

[0009] (3) Place the mixed powder in step 2) into a vacuum drying oven and dry at 60°C for 10 to 24 hours to obtain a dry mixed powder.

[0010] (4) The mixed powder in step 3) is cold pressed into a blank, and then the blank is subjected to spark plasma sintering or hot pressing sintering to obtain the target product (Ti 0.25 V 0.25 Nb0.25 Ta 0.25 ) 4 AlC 3 ceramics.

[0011] Spark plasma sintering is carried out in a vacuum environment with a vacuum degree of ≤5.0E0 Pa, a pressure of 30~40 MPa, and a sintering time of 15~30 min; the heating rate is 50~120℃ / min, and the sintering temperature is 1300~1400℃.

[0012] Hot pressing sintering is carried out in a vacuum environment with a vacuum degree of ≤10 -3 Pa, pressure is 30~40 MPa, sintering time is 1~2h; heating rate is 5~10 ℃ / min, sintering temperature is 1600~1650 ℃.

[0013] The synthesis mechanism of the present invention is as follows: As shown in the above formula, the 211-type MAX phase of the same element is supersaturated with Al element and lacks C element compared to the 413-type MAX phase, and the absence of C is conducive to the stable existence of the MAX phase. In addition, when the temperature reaches 650°C during the sintering process, the Al powder in the raw material volatilizes, and when the temperature rises to a certain level, the 211-type MAX phase can decompose, and the Al element decomposes and volatilizes from the material to generate a high-index MAX phase. Therefore, under a suitable sintering process, the decomposition of the 211-type high-entropy MAX phase and the volatilization of Al can be promoted to obtain the 413-type high-entropy MAX phase of the same element.

[0014] Parameters that promote Al volatilization and decomposition of the 211-type MAX phase include increasing the synthesis temperature and increasing the holding time. In Example 4 described later, the temperature is increased based on the comparative high entropy 211-type MAX phase synthesis process to obtain a 211-type and 413-type (mainly) MAX phase composite material, which means that the 211-type MAX phase has been decomposed. In Example 6, after further increasing the holding time based on Example 4, the 211-type MAX phase completely disappears, and a small amount of carbide phase appears, indicating that the 211 phase is completely decomposed, and even the 413-type MAX phase is slightly decomposed to form a carbide phase, which verifies the 413-type high entropy MAX phase synthesis mechanism proposed here.

[0015] The present invention has the following beneficial effects: The present invention provides a six-element layered high entropy MAX phase (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3The ceramic preparation method uses pure metal powder, or partial metal carbide powder, C powder as raw material. The design cost is lower than the existing process cost, the synthesis process is simpler, and there is no impurity element pollution in the synthetic target product. The prepared high-entropy MAX phase material has better tribological properties than the same element 211 type high-entropy MAX phase material in a wide temperature range. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 SEM microscopic morphology of ceramic materials of Example 1 and Example 2; Figure 2 XRD characterization results of ceramic materials of Example 1 and Example 2; Figure 3 Surface morphology of ceramic materials in Example 1 and Example 2; Figure 4 Example 3 Ceramic material XRD characterization results; Figure 5 Example 3 SEM cross section and cross-sectional characterization of ceramic materials; Figure 6 XRD characterization results of ceramic materials of Example 4 and Example 5; Figure 7 SEM cross-section and cross-sectional characterization images of ceramic materials of Example 4 and Example 5; Figure 8 Example 6 Ceramic material XRD characterization results; Fig. 9 Comparative Example (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 Microscopic morphology of AlC MAX phase ceramic material; Fig.10 Comparative Example (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 XRD analysis results of AlC MAX phase ceramic materials. DETAILED DESCRIPTION

[0017] In order to further explain the purpose, technical scheme and advantages of the present invention clearly, the following is a detailed description in conjunction with the embodiments. It should be understood that the embodiments herein are only used to explain the present invention and are not used to limit the scope of protection of the present invention. All technologies realized based on the above contents of the present invention are included in the scope of protection intended by the present invention.

[0018] The raw materials used in this embodiment are all commercially available products.

[0019] In the following embodiments and comparative examples of the present invention, a friction test was conducted using a Zhongke Kaihua HT-1200 friction tester to test the friction coefficient and wear rate of materials in the range of room temperature to 800°C, and the experimental conditions of the tests were the same.

[0020] Example 1 413 type six-element high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The preparation method of MAX phase ceramic material comprises the following steps: 1) Prepare ingredients according to the molar ratio of Ti:V:Nb:Ta:Al:C=0.5:0.5:0.5:0.5:1.2:0.9, with a total weight of 30g.

[0021] 2) The raw materials were placed in a zirconia-lined vacuum ball mill, with the mass percentage of zirconia balls: raw materials = 2:1; anhydrous ethanol was added as the ball milling medium, with the mass ratio of ethanol to raw materials being 40%; the ball mill was then evacuated and flushed with argon, and this operation was repeated 3 times; the ball mill was placed in a planetary ball mill, the ball milling speed was 280 rpm, and the ball milling time was 10 h to obtain a mixed powder.

[0022] 3) Place the mixed powder in step 2) in a vacuum drying oven and dry it at 60°C and a vacuum degree of -0.08MPa for 10 hours. Turn off the heating device and wait for the sample to cool to room temperature before taking it out.

[0023] 4) The mixed powder after drying in step 3) is cold pressed to obtain a blank, and the blank is placed in a corresponding graphite mold, and then spark plasma sintering is performed under a vacuum environment. The sintering process is as follows: the sintering furnace is evacuated to below 5.0E0 Pa at room temperature, the temperature is increased to 600°C at 120°C / min, and the temperature is increased to 1320°C at 50°C / min, and the temperature is kept for 20 minutes, and the pressure is loaded to 30 MPa. After the insulation is completed, the pressure is reduced and the temperature is lowered, and the sample is cooled with the furnace to prepare (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic material.

[0024] Example 2 413 type six-element high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC3 The preparation method of MAX phase ceramic material comprises the following steps: 1) Prepare ingredients according to the molar ratio of Ti:V:Nb:Ta:Al:C=0.5:0.5:0.5:0.5:1.2:0.9, with a total weight of 20g.

[0025] 2) The raw materials were placed in a zirconia-lined vacuum ball mill, with the mass percentage of zirconia balls: raw materials = 3:1; anhydrous ethanol was added as the ball milling medium, with the mass ratio of ethanol to raw materials being 40%; the ball mill was then evacuated and flushed with argon, and this operation was repeated 3 times; the ball mill was placed in a planetary ball mill, the ball milling speed was 300 rpm, and the ball milling time was 12 h to obtain a mixed powder.

[0026] 3) Place the mixed powder in step 2) in a vacuum drying oven and dry it at 60°C and a vacuum degree of -0.08MPa for 15 hours. Turn off the heating device and wait for the sample to cool to room temperature before taking it out.

[0027] 4) The mixed powder after drying in step 3) is cold pressed to obtain a blank, and the blank is placed in a corresponding graphite mold, and then spark plasma sintering is performed under a vacuum environment. The sintering process is as follows: the sintering furnace is evacuated to below 5.0E0 Pa at room temperature, the temperature is increased to 600°C at 120°C / min, and the temperature is increased to 1400°C at 50°C / min, and the temperature is kept for 20 minutes, and the pressure is loaded to 30 MPa. After the insulation is completed, the pressure is reduced and the temperature is lowered, and the sample is cooled with the furnace to prepare (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic material.

[0028] Example 3 413 type six-element high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The preparation method of MAX phase ceramic material comprises the following steps: 1) Prepare ingredients according to the molar ratio of Ti: V: NbC: TaC: Al=1: 1: 1: 1: 2.4, with a total weight of 30 g.

[0029] 2) The raw materials were placed in a zirconia-lined vacuum ball mill, with the mass percentage of zirconia balls: raw materials = 2: 1; anhydrous ethanol was added as the ball milling medium, with the mass ratio of ethanol to raw materials being 40%; the ball mill was then evacuated and flushed with argon, and this operation was repeated 3 times; the ball mill was placed in a planetary ball mill, the ball milling speed was 280 rpm, and the ball milling time was 12 h to obtain a mixed powder.

[0030] 3) Place the mixed powder in step 2) in a vacuum drying oven and dry it at 60°C and a vacuum degree of -0.08MPa for 15 hours. Turn off the heating device and wait for the sample to cool to room temperature before taking it out.

[0031] 4) The mixed powder after drying in step 3) is cold pressed to obtain a blank, and the blank is placed in a corresponding graphite mold, and then hot pressed and sintered in a vacuum environment. The sintering process is as follows: the sintering furnace is vacuumized to 10 at room temperature. -3 Pa, the temperature was raised to 1600°C at 10°C / min, and kept at this temperature for 90 min. The pressure was loaded at 30 MPa. After the heat preservation, the pressure and temperature were immediately reduced. The sample was cooled with the furnace to prepare (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic material.

[0032] Example 4 413 type six-element high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The preparation method of MAX phase ceramic material comprises the following steps: 1) Prepare ingredients according to the molar ratio of Ti: V: NbC: TaC: Al=1:1:1:1:2.4, with a total weight of 20g.

[0033] 2) The raw materials were placed in a zirconia-lined vacuum ball mill, with the mass percentage of zirconia balls: raw materials = 3:1; anhydrous ethanol was added as the ball milling medium, with the mass ratio of ethanol to raw materials being 40%; the ball mill was then evacuated and flushed with argon, and this operation was repeated 3 times; the ball mill was placed in a planetary ball mill, the ball milling speed was 280 rpm, and the ball milling time was 10 h to obtain a mixed powder.

[0034] 3) Place the mixed powder in step 2) in a vacuum drying oven and dry it at 60°C and a vacuum degree of -0.08MPa for 10 hours. Turn off the heating device and wait for the sample to cool to room temperature before taking it out.

[0035] 4) The mixed powder after drying in step 3) is cold pressed to obtain a blank, and the blank is placed in a corresponding graphite mold, and then hot pressed and sintered in a vacuum environment. The sintering process is as follows: the sintering furnace is vacuumized to 10 at room temperature. -3 Pa, the temperature was raised to 1600°C at 10°C / min, and then to 1650°C at 5°C / min, and kept at this temperature for 90 min. The loading pressure was 30 MPa, and the pressure and temperature were lowered immediately after the end of the heat preservation. The sample was cooled with the furnace to prepare (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic material.

[0036] Example 5 413 type six-element high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The preparation method of MAX phase ceramic material comprises the following steps: 1) Prepare the ingredients according to the molar ratio of Ti: V: NbC: TaC: Al=1: 1: 1: 1: 2.2, with a total weight of 30 g.

[0037] 2) Place the raw materials in a zirconia-lined vacuum ball mill, with the mass percentage of zirconia balls: raw materials = 2:1; add anhydrous ethanol as the ball milling medium, with the mass ratio of ethanol to raw materials being 40%; then evacuate the ball mill and flush it with argon, and repeat this operation 3 times; place the ball mill in a planetary ball mill, with the ball milling speed at 280 rpm and the ball milling time for 10 h to obtain a mixed powder.

[0038] 3) Place the mixed powder in step 2) in a vacuum drying oven and dry it at 60°C and a vacuum degree of -0.08MPa for 10 hours. Turn off the heating device and wait for the sample to cool to room temperature before taking it out.

[0039] 4) The mixed powder after drying in step 3) is cold pressed to obtain a blank, and the blank is placed in a corresponding graphite mold, and then hot pressed and sintered in a vacuum environment. The sintering process is as follows: the sintering furnace is vacuumized to 10 at room temperature. -3 Pa, the temperature was raised to 1600°C at 10°C / min, and then to 1650°C at 5°C / min, and kept at this temperature for 90 min. The loading pressure was 30 MPa, and the pressure and temperature were lowered immediately after the end of the heat preservation. The sample was cooled with the furnace to prepare (Ti 0.25 V 0.25 Nb0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic material.

[0040] Example 6 413 type six-element high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The preparation method of MAX phase ceramic material comprises the following steps: 1) Prepare ingredients according to the molar ratio of Ti: V: NbC: TaC: Al=1: 1: 1: 1: 2.4, with a total weight of 30 g.

[0041] 2) The raw materials were placed in a zirconia-lined vacuum ball mill, with the mass percentage of zirconia balls: raw materials = 2:1; anhydrous ethanol was added as the ball milling medium, with the mass ratio of ethanol to raw materials being 40%; the ball mill was then evacuated and flushed with argon, and this operation was repeated 3 times; the ball mill was placed in a planetary ball mill, the ball milling speed was 300 rpm, and the ball milling time was 10 h to obtain a mixed powder.

[0042] 3) Place the mixed powder in step 2) in a vacuum drying oven and dry it at 60°C and a vacuum degree of -0.08MPa for 10 hours. Turn off the heating device and wait for the sample to cool to room temperature before taking it out.

[0043] 4) The mixed powder after drying in step 3) is cold pressed to obtain a blank, and the blank is placed in a corresponding graphite mold, and then hot pressed and sintered in a vacuum environment. The sintering process is as follows: the sintering furnace is vacuumized to 10 at room temperature. -3 Pa, the temperature was raised to 1600℃ at 10℃ / min, and then raised to 1650℃ at 5℃ / min, and kept at this temperature for 120min. The loading pressure was 30MPa, and the pressure and temperature were lowered immediately after the end of the heat preservation. The sample was cooled with the furnace to prepare (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic material.

[0044] Comparative Example 211 type six-element high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 The preparation steps of AlC MAX phase ceramic materials are as follows: 1) Prepare ingredients according to the molar ratio of Ti:V:Nb:Ta:Al:C=0.5:0.5:0.5:0.5:1.2:0.9, with a total weight of 20g.

[0045] 2) The raw materials were placed in a zirconia-lined vacuum ball mill, with the mass percentage of zirconia balls: raw materials = 3:1; anhydrous ethanol was added as the ball milling medium, with the mass ratio of ethanol to raw materials being 40%; the ball mill was then evacuated and flushed with argon, and this operation was repeated 3 times; the ball mill was placed in a planetary ball mill, the ball milling speed was 280 rpm, and the ball milling time was 12 h to obtain a mixed powder.

[0046] 3) Place the mixed powder in step 2) in a vacuum drying oven and dry it at 60°C and a vacuum degree of -0.08MPa for 10 hours. Turn off the heating device and wait for the sample to cool to room temperature before taking it out.

[0047] 4) The mixed powder after drying in step 3) is cold pressed to obtain a blank, and the blank is placed in a corresponding graphite mold, and then hot pressed and sintered in a vacuum environment. The sintering process is as follows: the sintering furnace is vacuumized to 10 at room temperature. -3 Pa, the temperature was raised to 1500°C at 10°C / min, and kept at this temperature for 90 min. The pressure was loaded at 30 MPa. After the heat preservation, the pressure and temperature were immediately reduced. The sample was cooled with the furnace to prepare (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 AlC MAX phase ceramic material.

[0048] Product Characterization Example 1 and Example 2 (Ti) prepared by spark plasma sintering 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The SEM image of the fracture of MAX phase ceramic material is as follows Figure 1 As shown, the XRD spectrum is Figure 2 As shown, the surface morphology SEM image and EDS energy spectrum analysis element atomic ratio are as follows. Figure 3 And as shown in Table 1.

[0049] From the SEM fracture image, it can be seen that its microstructure is a typical MAX phase layered structure. From the XRD phase analysis, it can be seen that in addition to the 413 type high entropy MAX phase, there is also a 211 type high entropy MAX phase. Figure 3The area statistical analysis of the phase contrast of the two objects using ImageJ shows that the proportion of the 413 type high entropy MAX phase (bright contrast) in Example 1 is 70.6%, and the proportion of the 413 type high entropy MAX phase in Example 2 is 84%; EDS energy spectrum analysis, as shown in Table 1, the ratios of the elements at the M position of the two MAX phases are close to the same molar ratio, the molar ratio of the M position, A position, and X position elements of the 413 type is M: A: C=49.55:17.67:32.78≈4:1:3, and the molar ratio of the 211 type elements is M: A: C=45.24:26.60:21.57≈2:1:1, which is consistent with the XRD characterization results. Therefore, the 413 type high entropy (Ti) phase was successfully prepared. 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 Ceramic material with MAX phase as the main phase.

[0050] Table 1 (Ti prepared in Example 1 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 Atomic percentage table of MAX phase ceramic materials Example 3 The XRD characterization structure of the obtained high entropy ceramic is as follows Figure 4 As shown in the figure, the results show that the synthesized materials are 413 and 211 MAX phase ceramic materials. Figure 5 As shown, it is also a typical MAX phase layered structure. According to the phase contrast statistics, 413 type (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The proportion of MAX phase is 76.6%. 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 Ceramic material with MAX phase as the main phase.

[0051] The XRD characterization structure of the high entropy ceramics obtained in Example 4 and Example 5 is as follows: Figure 6 The results show that the synthesized material is a mixed ceramic material of 413 and 211 MAX phases. Figure 7As shown, the typical MAX phase layered structure, according to the phase contrast statistics of Example 4 413 type (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The proportion of MAX phase is 88%, and the 413 type (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The proportion of MAX phase is 86.3%. Therefore, the 413 type high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic material.

[0052] Example 6 XRD phase analysis Figure 8 As shown, under this process, 211 type (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 The AlCMAX phase disappears and the remaining phase is (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase, in addition there is a small amount of carbide phase, generating a nearly pure high entropy 413 type (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase.

[0053] In the comparative example (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 AlC MAX phase ceramic material microstructure SEM image, EDS spectrum analysis element atomic ratio and XRD spectrum as shown in Figures 9 and 10 And as shown in Table 2.

[0054] Table 2 Comparative Example Preparation (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2Atomic percentage table of AlC MAX phase ceramic materials From the SEM image, it can be seen that its microstructure is a typical MAX phase layered structure. EDS characterization shows that the ratio of each element in the M position is close to the same molar ratio, and the molar ratio of the elements in the M position, A position, and X position is M: A: C=47.11: 24.57: 21.35≈2: 1: 1. The XRD characterization results show that the diffraction peak is a high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 AlC MAX phase peak, almost no impurity peak, so the 211 type high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 2 AlC MAX phase ceramic material.

[0055] Performance Evaluation The wide temperature range tribological performance results of the high entropy MAX phase ceramic materials prepared in Example 6 and the comparative example under the same conditions are shown in Table 3 below. The friction conditions are a load of 5N and a grinding pair of Si 3 N 4 , reciprocating distance is 5 mm, and frequency is 300 rpm.

[0056] Table 3 Comparison of friction performance between Example 6 and comparative example It can be seen from the above table that Example 6 has better tribological properties, especially can effectively reduce the wear rate in the range of 400-800 ° C, that is, the 413 type high entropy (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 MAX phase ceramic materials have superior performance than 211 type MAX phase of the same element.

[0057] In summary, the six-element layered high entropy MAX phase (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 ) 4 AlC 3 The method for preparing ceramics, the prepared ceramic material is better than the 211 type (Ti 0.25 V 0.25 Nb 0.25 Ta0.25 ) 2 AlC MAX phase ceramic materials have better tribological properties in a wide temperature range. The raw materials are pure metal elements, graphite powder or single element carbide powder. The preparation process is simple, low-cost and reproducible. It is easy to scale up industrial production, laying the foundation for the synthesis of new high-entropy MAX phase materials and their applications in the field of friction.

[0058] The above only describes the embodiments of the present invention and is not intended to limit the present invention, which can be modified and varied in various ways. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A six-element layered high entropy MAX phase ceramic, characterized in that: The molecular formula is (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 )4AlC3.

2. A method for preparing the six-element layered high entropy MAX phase ceramic according to claim 1, characterized in that: The preparation steps are as follows: (1) M-site metal element powder, Al powder and C powder are mixed in proportion as raw materials, wherein the M-site metal powder includes Ti powder, V powder, Nb powder and Ta powder; or NbC or TaC carbide powder is used instead of Nb powder and Ta powder and then mixed with Ti powder, V powder and Al powder in proportion as raw materials; (2) ball milling the raw materials in step 1) for 10 to 12 hours under an argon atmosphere, adding 30% to 40% of the total weight of the raw materials in anhydrous ethanol as a ball milling medium, and grinding to obtain a mixed powder; (3) placing the mixed powder in step 2) in a vacuum drying oven and drying at 60° C. for 10 to 24 hours to obtain a dry mixed powder; (4) The mixed powder in step 3) is cold pressed into a blank, and then the blank is subjected to spark plasma sintering or hot pressing sintering to obtain the target product (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 )4AlC3 ceramics.

3. A method for preparing a six-element layered high entropy MAX phase ceramic as claimed in claim 2, characterized in that: In step 1), M-site Ti powder, V powder, Nb powder and Ta powder are mixed in equal molar ratios, and the molar ratio of M-site metal powder: Al powder: C powder is 2: (1.1~1.2): 0.9; the molar ratio of Ti powder: V powder: NbC powder: TaC powder: Al powder is 0.5: 0.5: 0.5: 0.5: (1.1~1.2).

4. A method for preparing a six-element layered high entropy MAX phase ceramic as claimed in claim 2, characterized in that: In step 1), the purity of the raw materials Ti powder, V powder, Nb powder, Ta powder, NbC powder, TaC powder, Al powder and C powder is ≥99%, and the powder particle size is not less than 325 mesh.

5. A method for preparing a six-element layered high entropy MAX phase ceramic as claimed in claim 2, characterized in that: In step 3), the ball-to-material ratio of the ball mill is (2~3): 1, and the ball mill speed is 200~400 rpm.

6. A method for preparing a six-element layered high entropy MAX phase ceramic as claimed in claim 2, characterized in that: In step 4), spark plasma sintering is carried out in a vacuum environment with a vacuum degree of ≤5.0E0 Pa, a pressure of 30-40 MPa, a sintering time of 15-30 min, a heating rate of 50-120 °C / min, and a sintering temperature of 1300-1400 °C.

7. A method for preparing a six-element layered high entropy MAX phase ceramic as claimed in claim 2, characterized in that: In step 4), hot pressing sintering is carried out in a vacuum environment with a vacuum degree of ≤10 -3 Pa, pressure is 30~40 MPa, sintering time is 1~2 h; heating rate is 5~10 ℃ / min, sintering temperature is 1600~1650 ℃.

8. A six-element layered high entropy MAX phase (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 )4AlC3 ceramic material.

9. A six-element layered high entropy MAX phase (Ti 0.25 V 0.25 Nb 0.25 Ta 0.25 )Application of 4AlC3 ceramic materials in high temperature resistant friction parts.

Citation Information

Patent Citations

  • MAX-phase high-entropy ceramic-based composite material and preparation method thereof

    CN113816746A

  • Easy-to-sinter wear-resistant friction-reducing high-entropy ceramic material and preparation method thereof

    CN114031406A

  • Medium-entropy MAX phase material, medium-entropy two-dimensional material and preparation method and application thereof

    CN114751750A

  • High- strength and heat-resisting high entropy alloy matrix composites and method of manufacturing the same

    KR1020170124441A

  • Method for obtaining carbide powder of a high-entropy alloy with a spherical particle shape

    RU2762897C1