Large-volume multifunctional mortar prepared from recycled micro powder and preparation method of large-volume multifunctional mortar
By using carbonized recycled concrete powder and hydrophobic modified surface coatings in foamed mortar, the problems of high cement consumption and poor durability are solved, low-carbon and durable multifunctional mortar are realized, and efficient recycling and utilization of construction solid waste is provided. plan.
Patent Information
- Application Number
- CN202411112384.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
Existing foamed mortar consumes a lot of cement during the production process, resulting in high carbon emissions. Due to the porous structure and high water absorption, the material has poor durability and is susceptible to dust pollution and water erosion.
Carbonized recycled concrete powder is used as auxiliary gelling material and surface coating. The durability of the mortar is improved through hydrophobic modification treatment, and greenhouse gas is sealed through carbonization reaction to reduce carbon emissions. At the same time, the surface coating is modified with titanate coupling agent. Improve the waterproof performance of the mortar.
It significantly improves the durability and low carbon footprint of the mortar, and provides a large-volume recycling solution that effectively absorbs construction solid waste, reduces the carbon emissions of foamed mortar production, and improves the corrosion resistance of the materials and Waterproof performance.
Smart Images

Figure CN118930307A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a multifunctional mortar utilizing recycled micropowder in large volume and a preparation method thereof. Background Art
[0002] As one of the most widely used building materials, the production of cement mortar contributes at least 8% of global carbon emissions and 3% of global energy consumption. Among them, polystyrene foam mortar, which uses polystyrene particles as fine aggregate and introduces bubbles into the slurry composed of cementitious materials, is often used as an exterior wall insulation material because of its thermal insulation, fire resistance and sound insulation properties.
[0003] However, the traditional preparation process of foamed mortar consumes a large amount of cement and produces a large amount of CO2 during its life cycle, which causes a joint loss of economic and environmental benefits; at the same time, due to the porous structure and high water absorption rate of foamed mortar, the mortar is easily affected by the adhesion of dust pollutants and the intrusion of water or corrosive media, resulting in poor material durability. Summary of the invention
[0004] The purpose of the present invention is to overcome at least one of the defects of the above-mentioned prior art and provide a multifunctional mortar and preparation method using recycled micropowder in large volume. The present invention provides a multifunctional mortar using recycled micropowder in large volume, including the mix ratio design and preparation process of the mortar body and the surface coating; wherein, the mortar mixing adopts a secondary mixing method, and the effective water-cement ratio is controlled by pre-wetting and stirring the binder and then adding the remaining components and stirring again; the mortar mix ratio adjusts the amount of carbonized recycled concrete powder based on different thermal insulation requirements; the surface coating powder is modified by ultrasonic activation method; the surface coating mix ratio adjusts the amount of titanate coupling agent based on different waterproof performance requirements.
[0005] The resource utilization of construction solid waste generated after the demolition of existing structures in urban renewal is a major measure for energy conservation and emission reduction in the construction industry. Among them, recycled concrete powder is a major product after the recycling of waste concrete. According to research, on the one hand, recycled concrete powder has a certain volcanic ash reaction and can be used as an auxiliary cementitious material to replace cement or fly ash; if the recycled concrete powder is pretreated by CO2 carbonization, it can not only improve its performance, but also use its carbonization reaction to seal greenhouse gases. Therefore, using carbonized recycled concrete powder as raw material will greatly reduce the carbon emissions of foamed mortar production. On the other hand, recycled concrete powder has the advantages of natural micro / nano structure and self-similarity with the substrate. After the hydrophilic hydroxyl groups on the surface of the powder are removed by a hydrophobic modifier to make it hydrophobic, it is very suitable as a surface coating to improve the durability of foamed mortar.
[0006] The present invention adopts carbonized recycled concrete powder as an auxiliary cementitious material and surface coating, while giving full play to the carbon absorption effect of the powder. The present invention obtains a multifunctional mortar with greatly improved durability and extremely low carbon footprint. At the same time, the present invention provides an application scheme that can effectively dispose of construction solid waste and recycle recycled concrete powder in large volumes.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] One of the purposes of the present invention is to provide a multifunctional mortar utilizing recycled micropowder in large volume, comprising the following components in parts by weight: 80-120 parts of fly ash; 100-125 parts of recycled micropowder; 25-30 parts of water glass; 6-8 parts of sodium hydroxide; 70-80 parts of water; 10-18 parts of polystyrene foam particles; 2-6 parts of polyvinyl alcohol fiber; 2-4 parts of foaming agent; 1-4 parts of water reducer; 1-4 parts of foam stabilizer; and 0.1-0.2 parts of titanate coupling agent.
[0009] Multifunctional mortar :
[0010] In the present invention, the fly ash is Class I fly ash with a density of no more than 2600 kg / m 3 ;
[0011] In the present invention, the regenerated micro powder is carbonized regenerated concrete powder, and the maximum particle size does not exceed 75 μm;
[0012] In the present invention, the water glass and sodium hydroxide are activators, and the sodium hydroxide is analytically pure; the polystyrene foam particles are fine aggregates, and the particle size is 0.15-4.75 mm;
[0013] In the present invention, the elongation at break of the polyvinyl alcohol fiber is not greater than 30%, and the tensile strength is not less than 1550 MPa;
[0014] In the present invention, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, and the water reducing efficiency is 20-25%;
[0015] In the present invention, the foaming agent is a hydrogen peroxide solution, the mass concentration of H2O2 is 30%, and it is analytically pure;
[0016] In the present invention, the foam stabilizer is one or more of hydroxypropyl methylcellulose, calcium stearate or tea saponin;
[0017] In the present invention, the titanate coupling agent is isopropyl tri(dioctyl pyrophosphate) titanate.
[0018] Multifunctional mortar :
[0019] In the present invention, the fly ash is preferably Class I fly ash, with a fineness of no more than 18.0 and a density of no more than 2600 kg / m 3 , meet the requirements of GB / T 1596-2017 "Fly ash for cement and concrete";
[0020] In the present invention, the regenerated micropowder is preferably carbonized regenerated concrete powder, the particle size of which is similar to that of fly ash and is not greater than 75 μm, meeting the requirements of JG-T 573-2020 "Regenerated Micropowder for Concrete and Mortar";
[0021] In the present invention, the mass fractions of SiO2 and Na2O in the water glass are not less than 25% and 8% respectively;
[0022] In the present invention, the sodium hydroxide is preferably analytically pure;
[0023] In the present invention, the water is ordinary tap water, and the temperature does not exceed 40°C;
[0024] In the present invention, the polystyrene foam particles have a particle size of 0.15-4.75 mm, a smooth spherical particle surface, and a bulk density of 14.80 kg / m 3 ;
[0025] In the present invention, the polyvinyl alcohol fiber has a length of 6 mm, a diameter of 18 μm, a tensile strength of 1600 MPa, and a specific gravity of 0.90;
[0026] In the present invention, the foaming agent is a hydrogen peroxide solution, which meets the requirements of JC / T 2199-2013 "Foaming Agent for Foamed Concrete";
[0027] In the present invention, the water reducer is a polycarboxylic acid high-efficiency water reducer with a water reduction efficiency of 20-25%, meeting the requirements of GB 50119-2013 "Technical Specifications for Application of Concrete Admixtures";
[0028] In the present invention, the foam stabilizer is preferably hydroxypropyl methylcellulose with a viscosity of 200,000;
[0029] In the present invention, the titanate coupling agent is preferably isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, a yellow transparent liquid with a density of 1060-1075 kg / m 3 , viscosity is 800-1400mPa·s, pH value is 2.0-4.0, which meets the requirements of GB / T35493-2017 "Titanate Coupling Agent".
[0030] The second object of the present invention is to provide a method for preparing a multifunctional mortar using a large volume of recycled micropowder as described above, comprising the following steps:
[0031] S1. Mixing fly ash and regenerated micro powder evenly to obtain a first mixture;
[0032] S2, adding polystyrene foam particles, polyvinyl alcohol fibers, water glass and sodium hydroxide consisting of an activator, a water reducer, a foam stabilizer and water to the first mixture, stirring evenly to obtain a second mixture;
[0033] S3, preparing an alkaline foaming solution, and using a foaming machine to make the alkaline foaming solution produce dense bubbles;
[0034] S4, adding the product obtained in S3 to the second mixture, stirring evenly, to obtain a freshly mixed foamed mortar;
[0035] S5. Spray the hydrophobic negative carbon coating onto the newly mixed foamed mortar to obtain a multifunctional mortar that utilizes a large volume of recycled micropowder.
[0036] 5. The method for preparing a multifunctional mortar using recycled micropowder in large volume according to claim 4, characterized in that in S5, the method for preparing the hydrophobic negative carbon coating comprises:
[0037] S51, mixing the recycled micro powder and water evenly, and then ultrasonically dispersing, adding a titanate coupling agent, stirring until uniform, sieving, and drying to obtain titanate-modified carbonized recycled concrete powder;
[0038] S52; Evenly mix the titanate-modified carbonized recycled concrete powder with water to obtain a hydrophobic negative carbon coating.
[0039] Furthermore, in S51, the mass ratio of the regenerated micro powder to water is 1 / 2-1 / 4; in S52, the mass ratio of the titanate-modified carbonized regenerated concrete powder to the water is 1 / 10-1 / 20.
[0040] Furthermore, in S51, the temperature of the ultrasonic dispersion is 65±3°C, and the drying is constant temperature drying at a temperature of at least 60°C.
[0041] Furthermore, in S51, after the titanate coupling agent is added, stirring is first performed at high speed and then at medium-high speed; the stirring speed of the high-speed stirring is 600-800 rpm; the stirring speed of the medium-high speed stirring is 300-500 rpm.
[0042] Furthermore, in S1 and S2, the stirring speed of the stirring process is 40-80 rpm; in S4, the stirring speed of the stirring process is 100-120 rpm.
[0043] Furthermore, in S3, the raw materials of the alkaline foaming agent solution include foaming agent, water glass, sodium hydroxide and water, and the mass ratio of the foaming agent to water is 1 / 10-1 / 20.
[0044] Furthermore, the prepared mortar has a compressive strength of not less than 1.0 MPa, a thermal conductivity of not more than 0.085 W (m·K), a softening coefficient of not less than 0.60, and a dry density of not more than 450 kg / m 3 , meeting the requirements of Type II mortar in GB / T 20473-2021 "Building Thermal Insulation Mortar".
[0045] Furthermore, the activation degree of the titanate-modified carbonized recycled concrete powder is not less than 75%; the solid content of the prepared mortar surface coating is not less than 70%, the impermeability performance is not less than P6 level, and it can pass the impermeability test with a test pressure of 0.3MPa and a test time of 30min, and meet the requirements of JGJ / T 220-2010 "Technical Code for Plastering Mortar".
[0046] Furthermore, the transportation and use of the prepared mortar are the same as those of conventional mortar. The above raw material usage ratio is for reference only and is determined according to the performance requirements of the actual situation during the specific design.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] (1) The present invention uses polystyrene foam particles as fine aggregate, and forms a low-carbon, early-strength foamed mortar by adding foam to an alkali-activated cementitious material, and ensures the anti-cracking performance of the mortar by adding polyvinyl alcohol fibers.
[0049] (2) The present invention utilizes the carbon absorption effect of recycled concrete powder through carbonization treatment, and further, on the one hand, the carbonized recycled concrete powder partially replaces the fly ash in the precursor, thereby reducing the carbon emissions from mortar production; on the other hand, the carbonized recycled concrete powder modified with a titanate coupling agent and having hydrophobicity is sprayed onto the surface of the freshly mixed mortar, thereby improving the corrosion resistance of the mortar.
[0050] (3) The present invention further provides a solution for disposing of construction solid waste and recycling large volumes of recycled micropowder to prepare multifunctional mortar, which has a relatively broad application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is a schematic flow chart of the method for preparing multifunctional mortar using recycled micropowder in large volume in the present invention. DETAILED DESCRIPTION
[0052] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0053] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. If no specific conditions are specified, the conventional conditions or the conditions recommended by the manufacturer shall be followed. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0054] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0055] With the rapid development of industrialization and urbanization, huge energy consumption and a large amount of solid waste are generated. Among the main solid wastes in my country, general industrial solid waste has the largest amount of production. In addition, the amount of construction waste in my country has accounted for 30% to 40% of the total urban waste. Although there are many methods for solid waste treatment at present, such as sanitary landfill, incineration, composting, etc. However, these methods will not only occupy a lot of land and spend a lot of construction funds, but also cause serious environmental pollution problems during the transportation and stacking process. In the process of urbanization, building solid waste has seriously affected the environment on which human beings depend for survival. At present, the utilization of solid waste is relatively small, and the domestic utilization rate is less than 10%. If the rich components in solid waste can be comprehensively utilized, it will create huge economic and environmental benefits.
[0056] The resource utilization of construction solid waste generated after the demolition of existing structures in urban renewal is a major measure for energy conservation and emission reduction in the construction industry. Among them, recycled concrete powder is a major product after the recycling of waste concrete. According to research, on the one hand, recycled concrete powder has a certain volcanic ash reaction and can be used as an auxiliary cementitious material to replace cement or fly ash; if the recycled concrete powder is pretreated by CO2 carbonization, it can not only improve its performance, but also use its carbonization reaction to seal greenhouse gases. Therefore, using carbonized recycled concrete powder as raw material will greatly reduce the carbon emissions of foamed mortar production. On the other hand, recycled concrete powder has the advantages of natural micro / nano structure and self-similarity with the substrate. After the hydrophilic hydroxyl groups on the surface of the powder are removed by a hydrophobic modifier to make it hydrophobic, it is very suitable as a surface coating to improve the durability of foamed mortar.
[0057] In summary, by using carbonized recycled concrete powder as an auxiliary cementitious material and surface coating and taking advantage of the carbon absorption effect of the powder, the present invention obtains a multifunctional mortar with greatly improved durability and extremely low carbon footprint; at the same time, the present invention provides an application scheme that can effectively dispose of construction solid waste and recycle recycled concrete powder in large volumes.
[0058] The invention provides a multifunctional mortar utilizing recycled micropowder in large volume, comprising the following components in parts by weight: 80-120 parts of fly ash; 100-125 parts of recycled micropowder; 25-30 parts of water glass; 6-8 parts of sodium hydroxide; 70-80 parts of water; 10-18 parts of polystyrene foam particles; 2-6 parts of polyvinyl alcohol fibers; 2-4 parts of foaming agent; 1-4 parts of water reducing agent; 1-4 parts of foam stabilizer; and 0.1-0.2 parts of titanate coupling agent.
[0059] In some embodiments of the present invention, the raw materials of the multifunctional mortar meet the following requirements:
[0060] The fly ash is Class I fly ash with a density of no more than 2600 kg / m 3 ;
[0061] The regenerated micro powder is carbonized regenerated concrete powder, and the maximum particle size does not exceed 75 μm;
[0062] The water glass and sodium hydroxide are activators, and the sodium hydroxide is analytically pure; the polystyrene foam particles are fine aggregates, and the particle size is 0.15-4.75 mm;
[0063] The breaking elongation of the polyvinyl alcohol fiber is not more than 30%, and the tensile strength is not less than 1550MPa;
[0064] The water reducing agent is a polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20-25%;
[0065] The foaming agent is a hydrogen peroxide solution, the H2O2 mass concentration is 30%, analytically pure;
[0066] The foam stabilizer is one or more of hydroxypropyl methylcellulose, calcium stearate or tea saponin;
[0067] The titanate coupling agent is isopropyl tri(dioctyl pyrophosphate) titanate.
[0068] More preferably, in some embodiments of the present invention, the raw materials of the multifunctional mortar meet the following requirements:
[0069] The fly ash is preferably Class I fly ash, with a fineness of no more than 18.0 and a density of no more than 2600 kg / m 3 , meet the requirements of GB / T1596-2017 "Fly ash for cement and concrete";
[0070] The regenerated micropowder is preferably carbonized regenerated concrete powder, the particle size of which is similar to that of fly ash and is not greater than 75 μm, meeting the requirements of JG-T 573-2020 "Regenerated Micropowder for Concrete and Mortar";
[0071] The mass fractions of SiO2 and Na2O in the water glass are not less than 25% and 8% respectively;
[0072] The sodium hydroxide is preferably analytically pure;
[0073] The water is ordinary tap water, the temperature of which does not exceed 40°C;
[0074] The polystyrene foam particles have a particle size of 0.15-4.75 mm, a smooth spherical particle surface, and a bulk density of 14.80 kg / m 3 ;
[0075] The polyvinyl alcohol fiber has a length of 6 mm, a diameter of 18 μm, a tensile strength of 1600 MPa, and a specific gravity of 0.90;
[0076] The foaming agent is a hydrogen peroxide solution, which meets the requirements of JC / T 2199-2013 "Foaming Agent for Foamed Concrete";
[0077] The water reducer is a polycarboxylic acid high-efficiency water reducer with a water reduction efficiency of 20-25%, meeting the requirements of GB 50119-2013 "Technical Specifications for Application of Concrete Admixtures";
[0078] The foam stabilizer is preferably hydroxypropyl methylcellulose with a viscosity of 200,000;
[0079] The titanate coupling agent is preferably isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, a yellow transparent liquid with a density of 1060-1075 kg / m 3 , viscosity is 800-1400, pH value is 2.0-4.0, which meets the requirements of GB / T 35493-2017 "Titanate Coupling Agent".
[0080] The present invention also provides a method for preparing the multifunctional mortar using the recycled micropowder in large volume as described above, comprising the following steps:
[0081] S1. Mixing fly ash and regenerated micro powder evenly to obtain a first mixture;
[0082] S2, adding polystyrene foam particles, polyvinyl alcohol fibers, water glass and sodium hydroxide consisting of an activator, a water reducer, a foam stabilizer and water to the first mixture, stirring evenly to obtain a second mixture;
[0083] S3, preparing an alkaline foaming solution, and using a foaming machine to make the alkaline foaming solution produce dense bubbles;
[0084] S4, adding the product obtained in S3 to the second mixture, stirring evenly, to obtain a freshly mixed foamed mortar;
[0085] S5. Spray the hydrophobic negative carbon coating onto the newly mixed foamed mortar to obtain a multifunctional mortar that utilizes a large volume of recycled micropowder.
[0086] In some embodiments of the present invention, in S5, the method for preparing the hydrophobic negative carbon coating comprises:
[0087] S51, mixing the recycled micro powder and water evenly, and then ultrasonically dispersing, adding a titanate coupling agent, stirring until uniform, sieving, and drying to obtain titanate-modified carbonized recycled concrete powder;
[0088] S52; Evenly mix the titanate-modified carbonized recycled concrete powder with water to obtain a hydrophobic negative carbon coating.
[0089] In some embodiments of the present invention, in S51, the mass ratio of the regenerated micropowder to water is 1 / 2-1 / 4; in S52, the mass ratio of the titanate-modified carbonized regenerated concrete powder to the water is 1 / 10-1 / 20.
[0090] In some embodiments of the present invention, in S51, the temperature of the ultrasonic dispersion is 65±3°C, and the drying is constant temperature drying at a temperature of at least 60°C.
[0091] In some embodiments of the present invention, in S51, after adding the titanate coupling agent, stirring is first performed at high speed and then at medium-high speed; the stirring speed of the high-speed stirring is 600-800 rpm; the stirring speed of the medium-high speed stirring is 300-500 rpm.
[0092] In some embodiments of the present invention, in S1 and S2, the stirring speed of the stirring process is 40-80 rpm; in S4, the stirring speed of the stirring process is 100-120 rpm.
[0093] In some embodiments of the present invention, in S3, the raw materials of the alkaline foaming agent solution include foaming agent, water glass, sodium hydroxide and water, and the mass ratio of the foaming agent to water is 1 / 10-1 / 20.
[0094] In some embodiments of the present invention, the prepared mortar has a compressive strength of not less than 1.0 MPa after hardening, a thermal conductivity of not more than 0.085 W (m·K), a softening coefficient of not less than 0.60, and a dry density of not more than 450 kg / m 3 , meeting the requirements of Type II mortar in GB / T 20473-2021 "Building Thermal Insulation Mortar".
[0095] In some embodiments of the present invention, the activation degree of the titanate-modified carbonized recycled concrete powder is not less than 75%; the solid content of the prepared mortar surface coating is not less than 70%, the impermeability performance is not less than P6 level, and it can pass the impermeability test with a test pressure of 0.3MPa and a test time of 30min, and meet the requirements of JGJ / T 220-2010 "Technical Code for Plastering Mortar".
[0096] In some embodiments of the present invention, the transportation and use of the prepared mortar are the same as those of conventional mortar. The above raw material usage ratio is for reference only and is determined according to the performance requirements of the actual situation during the specific design.
[0097] Comparative Example 1 :
[0098] A multifunctional mortar without carbonized recycled concrete powder and without spraying surface coating comprises the following steps:
[0099] 1) Select 200 parts of fly ash and add it into a mixer, and dry mix it at a low speed of 60r / min for 1 minute;
[0100] 2) Slowly add 14 parts of dried polystyrene foam particles, 22 parts of water glass, 5 parts of sodium hydroxide, 1 part of water reducer, 1 part of foam stabilizer and 76 parts of water into the mixer, and gradually add 3 parts of loose polyvinyl alcohol fiber, stir at a low speed of 60r / min for 3 minutes until the above components are evenly mixed;
[0101] 3) Add 6 parts of water glass and 2 parts of sodium hydroxide into a container, dissolve them with an appropriate amount of water, add 3 parts of foaming agent, pour the solution into a 3.7kw air compressor, set the air pressure to -0.4 atmospheres, pass high-pressure airflow to make the solution pass through a special foaming cylinder for 1 minute until dense and uniform foam appears, and then directly pass it into a blender;
[0102] 4) The mixer is kept stirring at 120r / min for 2 minutes until all materials are evenly mixed;
[0103] 5) The prepared foamed mortar molded sample was cured in a standard curing room for 1 day and then demolded, and then the demolded sample was placed in a standard curing room for further curing for 6 days to obtain a multifunctional mortar that does not contain carbonized recycled concrete powder and is not sprayed with surface coating.
[0104] Comparative Example 2 :
[0105] A multifunctional mortar containing carbonized recycled concrete powder and not sprayed with surface coating comprises the following steps:
[0106] 1) Select unmodified recycled concrete powder produced by a waste concrete processing plant, sieve out materials with a particle size of less than 75 μm through a sorting machine, remove excess inorganic impurities, and send them to a dryer with a set temperature of 105°C for continuous drying for 24 hours. Then, place the dried powder in layers in a carbonization vacuum pressure reactor with a set pressure of 0.4 MPa, place a certain amount of desiccant on the surface, tighten the high-strength fixing bolts, evacuate the reactor to a vacuum state, and continuously introduce high-purity CO2 gas for more than 60 minutes. Finally, take out the powder and use it as carbonization recycled concrete powder for standby use;
[0107] 2) Select 100 parts of fly ash and 100 parts of carbonized recycled concrete powder, add them into a mixer in sequence, and dry mix at a low speed of 60r / min for 1 minute until the above components are evenly mixed;
[0108] 3) Slowly add 14 parts of dried polystyrene foam particles, 22 parts of water glass, 5 parts of sodium hydroxide, 1 part of water reducer, 1 part of foam stabilizer and 76 parts of water into the mixer, and gradually add 3 parts of loose polyvinyl alcohol fibers, stir at a low speed of 60r / min for 3 minutes until the above components are evenly mixed;
[0109] 4) Add 6 parts of water glass and 2 parts of sodium hydroxide to a container, dissolve them with an appropriate amount of water, add 3 parts of foaming agent, pour the solution into a 3.7kw air compressor, set the air pressure to -0.4 atmospheres, pass high-pressure airflow to make the solution pass through a special foaming cylinder for 1 minute until dense and uniform foam appears, and then directly pass it into a blender;
[0110] 5) The mixer is kept stirring at a high speed of 120 r / min for 2 min until all materials are evenly mixed;
[0111] 6) The prepared foamed mortar molded sample was cured in a standard curing room for 1 day and then demolded, and then the demolded sample was placed in a standard curing room for further curing for 6 days to obtain a multifunctional mortar containing carbonized recycled concrete powder and without spraying surface coating.
[0112] Comparative Example 3 :
[0113] A multifunctional mortar without carbonized recycled concrete powder and sprayed with surface coating comprises the following steps:
[0114] 1) Select 200 parts of fly ash, add it into a mixer, and dry mix it at a low speed of 60r / min for 1 minute;
[0115] 2) Slowly add 14 parts of dried polystyrene foam particles, 22 parts of water glass, 5 parts of sodium hydroxide, 1 part of water reducer, 1 part of foam stabilizer and 76 parts of water into the mixer, and gradually add 3 parts of loose polyvinyl alcohol fiber, stir at a low speed of 60r / min for 3 minutes until the above components are evenly mixed;
[0116] 3) Add 6 parts of water glass and 2 parts of sodium hydroxide into a container, dissolve them with an appropriate amount of water, add 3 parts of foaming agent, pour the solution into a 3.7kw air compressor, set the air pressure to -0.4 atmospheres, pass high-pressure airflow to make the solution pass through a special foaming cylinder for 1 minute until dense and uniform foam appears, and then directly pass it into a blender;
[0117] 4) The mixer is kept stirring at 120r / min for 2 minutes until all materials are evenly mixed;
[0118] 5) 20 parts of carbonized recycled concrete powder and 6 parts of water were selected, mixed evenly and added to an ultrasonic disperser, and the temperature was controlled to operate at 68°C for 30 minutes; the suspension after ultrasonic dispersion and 0.2 parts of titanate coupling agent were selected and added to a high-speed mixer, stirred at a high speed of 700 r / min for 15 minutes, and then changed to a medium-high speed of 400 r / min for 15 minutes; after filtering the obtained suspension, it was sent to a drying machine set at a temperature of 60°C and continuously dried to constant weight to obtain titanate-modified carbonized recycled concrete powder;
[0119] 6) Select 20 parts of titanate-modified carbonized recycled concrete powder and 1 part of water, mix well and spray them evenly on the surface of the freshly mixed foamed mortar as a mortar surface coating, cure the prepared molded sample in a standard curing room for 1 day and then demold, then place the demolded sample in a standard curing room for another 6 days, and obtain a multifunctional mortar without carbonized recycled concrete powder and sprayed surface coating.
[0120] Embodiment 1:
[0121] See also Figure 1 , a multifunctional mortar I containing carbonized recycled concrete powder and sprayed surface coating, comprising the following steps:
[0122] 1) Select unmodified recycled concrete powder produced by a waste concrete processing plant, sieve out materials with a particle size of less than 75 μm through a sorting machine, remove excess inorganic impurities, and send them to a dryer with a set temperature of 105°C for continuous drying for 24 hours. Then, place the dried powder in layers in a carbonization vacuum pressure reactor with a set pressure of 0.4 MPa, place a certain amount of desiccant on the surface, tighten the high-strength fixing bolts, evacuate the reactor to a vacuum state, and continuously introduce high-purity CO2 gas for more than 60 minutes. Finally, take out the powder and use it as carbonization recycled concrete powder for standby use;
[0123] 3) Select 100 parts of fly ash and 100 parts of carbonized recycled concrete powder, add them into the mixer in sequence, and dry mix at a low speed of 60r / min for 1 minute until the above components are evenly mixed;
[0124] 3) Slowly add 14 parts of dried polystyrene foam particles, 22 parts of water glass, 5 parts of sodium hydroxide, 1 part of water reducer, 1 part of foam stabilizer and 76 parts of water into the mixer, and gradually add 3 parts of loose polyvinyl alcohol fibers, stir at a low speed of 60r / min for 3 minutes until the above components are evenly mixed;
[0125] 4) Add 6 parts of water glass and 2 parts of sodium hydroxide to a container, dissolve them with an appropriate amount of water, add 3 parts of foaming agent, pour the solution into a 3.7kw air compressor, set the air pressure to -0.4 atmospheres, pass high-pressure airflow to make the solution pass through a special foaming cylinder for 1 minute until dense and uniform foam appears, and then directly pass it into a blender;
[0126] 5) The mixer is kept stirring at 120r / min for 2 minutes until all materials are evenly mixed;
[0127] 6) 20 parts of carbonized recycled concrete powder and 6 parts of water were selected, mixed evenly and added to an ultrasonic disperser, and the temperature was controlled to operate at 68°C for 30 minutes; the suspension after ultrasonic dispersion and 0.2 parts of titanate coupling agent were selected and added to a high-speed mixer, stirred at a high speed of 700 r / min for 15 minutes, and then changed to a medium-high speed of 400 r / min for 15 minutes; after filtering the obtained suspension, it was sent to a drying machine set at a temperature of 60°C and continuously dried to constant weight to obtain titanate-modified carbonized recycled concrete powder;
[0128] 7) Select 20 parts of titanate-modified carbonized recycled concrete powder and 1 part of water, mix well and spray them evenly on the surface of the freshly mixed foamed mortar as a mortar surface coating, cure the prepared molded sample in a standard curing room for 1 day and then demold, then place the demolded sample in a standard curing room for another 6 days, and obtain a multifunctional mortar without carbonized recycled concrete powder and sprayed surface coating.
[0129] Example 2
[0130] See also Figure 1 , a multifunctional mortar II containing carbonized recycled concrete powder and sprayed surface coating, comprising the following steps:
[0131] 1) Select unmodified recycled concrete powder produced by a waste concrete processing plant, sieve out materials with a particle size of less than 75 μm through a sorting machine, remove excess inorganic impurities, and send them to a dryer with a set temperature of 105°C for continuous drying for 24 hours. Then, place the dried powder in layers in a carbonization vacuum pressure reactor with a set pressure of 0.4 MPa, place a certain amount of desiccant on the surface, tighten the high-strength fixing bolts, evacuate the reactor to a vacuum state, and continuously introduce high-purity CO2 gas for more than 60 minutes. Finally, take out the powder and use it as carbonization recycled concrete powder for standby use;
[0132] 2) Select 80 parts of fly ash and 80 parts of carbonized recycled concrete powder, add them into the mixer in sequence, and dry mix at a low speed of 60r / min for 1 minute until the above components are evenly mixed;
[0133] 3) Slowly add 10 parts of dried polystyrene foam particles, 20 parts of water glass, 4 parts of sodium hydroxide, 1 part of water reducer, 1 part of foam stabilizer and 64 parts of water into the mixer, and gradually add 2 parts of loose polyvinyl alcohol fibers, stir at a low speed of 60r / min for 3 minutes until the above components are evenly mixed;
[0134] 4) Add 5 parts of water glass and 2 parts of sodium hydroxide to a container, dissolve them with an appropriate amount of water, add 2 parts of foaming agent, pour the solution into a 3.7kw air compressor, set the air pressure to -0.4 atmospheres, pass high-pressure airflow to make the solution pass through a special foaming cylinder for 1 minute until dense and uniform foam appears, and then directly pass it into a blender;
[0135] 5) The mixer is kept stirring at a high speed of 120 r / min for 2 min until all materials are evenly mixed;
[0136] 6) 20 parts of carbonized recycled concrete powder and 5 parts of water were selected, mixed evenly and added to an ultrasonic disperser, and the temperature was controlled to operate at 68°C for 30 minutes; the suspension after ultrasonic dispersion and 0.1 parts of titanate coupling agent were added to a high-speed mixer, stirred at a high speed of 700 r / min for 15 minutes, and then changed to a medium-high speed of 400 r / min for 15 minutes; after filtering the obtained suspension, it was sent to a drying machine set at a temperature of 60°C and continuously dried to constant weight to obtain titanate-modified carbonized recycled concrete powder;
[0137] 7) Select 20 parts of titanate-modified carbonized recycled concrete powder and 1 part of water, mix well and spray them evenly on the surface of the freshly mixed foamed mortar as a mortar surface coating, cure the prepared molded sample in a standard curing room for 1 day and then demold, then place the demolded sample in a standard curing room for another 6 days, and obtain a multifunctional mortar without carbonized recycled concrete powder and sprayed surface coating.
[0138] Example 3
[0139] See also Figure 1 , a multifunctional mortar III containing carbonized recycled concrete powder and sprayed surface coating, comprising the following steps:
[0140] 1) Select unmodified recycled concrete powder produced by a waste concrete processing plant, sieve out materials with a particle size of less than 75 μm through a sorting machine, remove excess inorganic impurities, and send them to a dryer with a set temperature of 105°C for continuous drying for 24 hours. Then, place the dried powder in layers in a carbonization vacuum pressure reactor with a set pressure of 0.4 MPa, place a certain amount of desiccant on the surface, tighten the high-strength fixing bolts, evacuate the reactor to a vacuum state, and continuously introduce high-purity CO2 gas for more than 60 minutes. Finally, take out the powder and use it as carbonization recycled concrete powder for standby use;
[0141] 2) Select 120 parts of fly ash and 105 parts of carbonized recycled concrete powder, add them into the mixer in sequence, and dry mix at a low speed of 60r / min for 1 minute until the above components are evenly mixed;
[0142] 3) Slowly add 18 parts of dried polystyrene foam particles, 22 parts of water glass, 6 parts of sodium hydroxide, 4 parts of water reducer, 4 parts of foam stabilizer and 74 parts of water into the mixer, and gradually add 6 parts of loose polyvinyl alcohol fibers, stir at a low speed of 60r / min for 3 minutes until the above components are evenly mixed;
[0143] 4) Add 8 parts of water glass and 2 parts of sodium hydroxide to a container, dissolve them with an appropriate amount of water, add 4 parts of foaming agent, pour the solution into a 3.7kw air compressor, set the air pressure to -0.4 atmospheres, pass high-pressure airflow to make the solution pass through a special foaming cylinder for 1 minute until dense and uniform foam appears, and then directly pass it into a blender;
[0144] 5) The mixer is kept stirring at 120r / min for 2 minutes until all materials are evenly mixed;
[0145] 6) 20 parts of carbonized recycled concrete powder and 5 parts of water were selected, mixed evenly and added to an ultrasonic disperser, and the temperature was controlled to operate at 68°C for 30 minutes; the suspension after ultrasonic dispersion and 0.2 parts of titanate coupling agent were added to a high-speed mixer, stirred at a high speed of 700 r / min for 15 minutes, and then changed to a medium-high speed of 400 r / min for 15 minutes; after filtering the obtained suspension, it was sent to a drying machine set at a temperature of 60°C and continuously dried to constant weight to obtain titanate-modified carbonized recycled concrete powder;
[0146] 7) Select 20 parts of titanate-modified carbonized recycled concrete powder and 1 part of water, mix well and spray them evenly on the surface of the freshly mixed foamed mortar as a mortar surface coating, cure the prepared molded sample in a standard curing room for 1 day and then demold, then place the demolded sample in a standard curing room for another 6 days, and obtain a multifunctional mortar without carbonized recycled concrete powder and sprayed surface coating.
[0147] The above-mentioned comparative examples 1-3 and embodiment 1 respectively prepared multifunctional mortar without carbonized recycled concrete powder and without spraying surface coating, multifunctional mortar with carbonized recycled concrete powder and without spraying surface coating, multifunctional mortar without carbonized recycled concrete powder and spraying surface coating, and multifunctional mortar with carbonized recycled concrete powder and spraying surface coating.
[0148] In particular, the mechanical properties and thermal insulation properties of the above-mentioned embodiments are respectively carried out in accordance with the requirements of GB / T 5486-2008 "Test methods for inorganic rigid thermal insulation products" and GB / T 10294-2008 "Determination of steady-state thermal resistance and related properties of thermal insulation materials". The test results are shown in Table 2, where, compared with Example 1 (control group), when 50% of fly ash is replaced by carbonized recycled concrete powder and the surface coating is sprayed, the CO2 emission of the multifunctional mortar is reduced by 9.4%, and it also has more excellent mechanical properties and other functionalities, meeting the requirements of GB / T 20473-2021 "Building thermal insulation mortar".
[0149] Table 2 Comparison of mortar properties prepared in Comparative Examples 1-3 and Example 1
[0150]
[0151]
[0152] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A multifunctional mortar utilizing recycled micropowder in large volume, characterized in that: The composition comprises the following components in parts by weight:
2. The multifunctional mortar using recycled micro powder in large volume according to claim 1, characterized in that: The multifunctional mortar meets at least one of the following conditions: ① The fly ash is Grade I fly ash with a density not greater than 2600kg / m 3 ; ② The regenerated micro powder is carbonized regenerated concrete powder, and the maximum particle size does not exceed 75 μm; ③ The water glass and sodium hydroxide are activators, and the sodium hydroxide is analytically pure; the polystyrene foam particles are fine aggregates, and the particle size is 0.15-4.75mm; ④ The elongation at break of the polyvinyl alcohol fiber is not greater than 30%, and the tensile strength is not less than 1550MPa; ⑤ The water reducing agent is a polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20-25%; ⑥ The foaming agent is a hydrogen peroxide solution, the mass concentration of H2O2 is 30%, analytical grade; ⑨The foam stabilizer is one or more of hydroxypropyl methylcellulose, calcium stearate or tea saponin; ⑩ The titanate coupling agent is isopropyl tri(dioctyl pyrophosphate) titanate.
3. The multifunctional mortar using recycled micro powder in large volume according to claim 1, characterized in that: The multifunctional mortar meets at least one of the following conditions: ① The fly ash is preferably Class I fly ash, with a fineness of no more than 18.0 and a density of no more than 2600 kg / m 3 , meet the requirements of GB / T1596-2017 "Fly ash for cement and concrete"; ② The regenerated micropowder is preferably carbonized regenerated concrete powder, the particle size of which is similar to that of fly ash and is not greater than 75 μm, meeting the requirements of JG-T 573-2020 "Regenerated Micropowder for Concrete and Mortar"; ③ The mass fractions of SiO2 and Na2O in the water glass are not less than 25% and 8% respectively; ④ The sodium hydroxide is preferably analytically pure; ⑤ The water is ordinary tap water, the temperature of which does not exceed 40°C; ⑥ The polystyrene foam particles have a particle size of 0.15-4.75 mm, a smooth spherical particle surface, and a bulk density of 14.80 kg / m 3 ; ⑦ The polyvinyl alcohol fiber has a length of 6 mm, a diameter of 18 μm, a tensile strength of 1600 MPa, and a specific gravity of 0.90; ⑧ The foaming agent is a hydrogen peroxide solution, which meets the requirements of JC / T 2199-2013 "Foaming Agent for Foamed Concrete"; ⑨ The water reducer is a polycarboxylic acid high-efficiency water reducer with a water reduction efficiency of 20-25%, meeting the requirements of GB 50119-2013 "Technical Specifications for Application of Concrete Admixtures"; ⑩ The foam stabilizer is preferably hydroxypropyl methylcellulose with a viscosity of 200,000; The titanate coupling agent is preferably isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, a yellow transparent liquid with a density of 1060-1075 kg / m 3 , viscosity is 800-1400mPa·s, pH value is 2.0-4.0, which meets the requirements of GB / T 35493-2017 "Titanate Coupling Agent".
4. The method for preparing multifunctional mortar using recycled micropowder in large volume as claimed in any one of claims 1 to 3, characterized in that: The steps include: S1. Mixing fly ash and regenerated micro powder evenly to obtain a first mixture; S2, adding polystyrene foam particles, polyvinyl alcohol fibers, water glass and sodium hydroxide consisting of an activator, a water reducer, a foam stabilizer and water to the first mixture, stirring evenly to obtain a second mixture; S3, preparing an alkaline foaming solution, and using a foaming machine to make the alkaline foaming solution produce dense bubbles; S4, adding the product obtained in S3 to the second mixture, stirring evenly, to obtain a freshly mixed foamed mortar; S5. Spray the hydrophobic negative carbon coating onto the newly mixed foamed mortar to obtain a multifunctional mortar that utilizes a large volume of recycled micropowder.
5. The method for preparing a multifunctional mortar using recycled micropowder in large volume according to claim 4, characterized in that: In S5, the preparation method of the hydrophobic negative carbon coating comprises: S51, mixing the recycled micro powder and water evenly, and then ultrasonically dispersing, adding a titanate coupling agent, stirring until uniform, sieving, and drying to obtain titanate-modified carbonized recycled concrete powder; S52; Evenly mix the titanate-modified carbonized recycled concrete powder with water to obtain a hydrophobic negative carbon coating.
6. The method for preparing a multifunctional mortar using recycled micropowder in large volume according to claim 5, characterized in that: In S51, the mass ratio of the regenerated micropowder to water is 1 / 2-1 / 4; In S52, the mass ratio of the titanate-modified carbonized recycled concrete powder to the water is 1 / 10-1 / 20.
7. The method for preparing a multifunctional mortar using recycled micropowder in large volume according to claim 5, characterized in that: In S51, the temperature of the ultrasonic dispersion is 65±3°C, and the drying is constant temperature drying at a temperature of at least 60°C.
8. The method for preparing a multifunctional mortar using recycled micropowder in large volume according to claim 5, characterized in that: In S51, after adding the titanate coupling agent, stirring is first performed at high speed, and then at medium-high speed; The stirring speed of the high-speed stirring is 600-800 rpm; the stirring speed of the medium-high-speed stirring is 300-500 rpm.
9. The method for preparing a multifunctional mortar using recycled micropowder in large volume according to claim 4, characterized in that: In S1 and S2, the stirring speed of the stirring process is 40-80 rpm; in S4, the stirring speed of the stirring process is 100-120 rpm.
10. The method for preparing a multifunctional mortar using recycled micropowder in large volume according to claim 4, characterized in that: In S3, the raw materials of the alkaline foaming agent solution include foaming agent, water glass, sodium hydroxide and water, and the mass ratio of the foaming agent to water is 1 / 10-1 / 20.
Citation Information
Patent Citations
Concrete and preparation method thereof
CN111153662A
Alkali-activated regenerated micro-powder foam concrete and preparation method thereof
CN112062533A
Method for completely carbonizing regenerated powder
CN114620963A
Alkali-activated thermal insulation mortar utilizing regenerated micro powder on large scale and preparation method of alkali-activated thermal insulation mortar
CN117024109A
Foam concrete containing construction waste regenerated micro powder and preparation method thereof
CN117088708A