Ultrafast-drying hydroxy acrylic resin, preparation method thereof and application of ultrafast-drying hydroxy acrylic resin in polyurethane varnish

By using hydroxyethyl acrylate and hydroxyethyl methacrylate in hydroxyacrylate in hydroxyacrylate and combination with other monomers and specific additives, an ultra-fast drying resin was prepared for polyurethane varnish, which solved the problem of traditional resin drying The problems of slow speed and insufficient environmental performance achieve high-performance and environmentally friendly coating effects.

CN118930720APending Publication Date: 2024-11-12QINGYUAN HUAYUAN INST OF SCI & TECH COLLABORATIVE INNOVATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411171715.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional hydroxyacrylic resins dry slowly in harsh environments such as low temperature and high humidity, which affects construction efficiency and coating quality, and also needs to meet increasingly stringent environmental protection requirements.

Method used

Hydroxyethyl acrylate and hydroxyethyl methacrylate are used as highly active hydroxyl monomers and acrylate and methacrylic monomers, combining specific proportions of catalysts, initiators, chain transfer agents and functional additives. Ultra-fast dry hydroxyacrylic resin is prepared and combined with isocyanate curing agent for use in polyurethane varnish.

Benefits of technology

It realizes the ultra-fast drying characteristics of the coating, improves weather resistance, chemical corrosion resistance and hardness, meets the use requirements in harsh environments, and has good environmental protection performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005009469090000071
    Figure BDA0005009469090000071
  • Figure BDA0005009469090000081
    Figure BDA0005009469090000081
  • Figure BDA0005009469090000082
    Figure BDA0005009469090000082
Patent Text Reader

Abstract

The invention discloses an ultrafast-drying hydroxy acrylic resin, a preparation method thereof and an application of the ultrafast-drying hydroxy acrylic resin in polyurethane varnish, and relates to the technical field of coatings. The invention relates to a preparation method of ultrafast-drying hydroxy acrylic resin, which comprises the following steps: (1) uniformly mixing a high-activity hydroxyl monomer, an acrylate monomer, a methacrylic acid monomer and a solvent to obtain a premixed solution; (2) adding an initiator, a chain transfer agent and a functional aid into the premixed solution, and reacting at 140-160 DEG C for 2-3 hours; and (3) cooling to 60-70 DEG C, adding a catalyst, uniformly mixing, and filtering to obtain the ultrafast-drying hydroxy acrylic resin. The super-quick-drying hydroxy acrylic resin has super-quick-drying performance, and when the super-quick-drying hydroxy acrylic resin is added into polyurethane varnish, a coating has excellent weather resistance, chemical corrosion resistance, hardness and decoration performance, and can meet the use requirements in various severe environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to an ultra-fast drying hydroxy acrylic resin and a preparation method thereof and application of the resin in polyurethane varnish. Background Art

[0002] Although traditional hydroxy acrylic resin coatings have good weather resistance, chemical corrosion resistance and decorative properties, in practical applications, especially in harsh environments such as low temperature and high humidity, they dry slowly and their hardness rises slowly, affecting construction efficiency and coating quality. In addition, with increasingly stringent environmental regulations, the coatings industry has increasingly higher requirements for environmental performance. Therefore, the development of a hydroxy acrylic resin and polyurethane varnish that has both high performance and ultra-fast drying characteristics and meets environmental requirements has important practical application value. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an ultra-fast drying hydroxy acrylic resin and a preparation method thereof and an application thereof in polyurethane varnish. The ultra-fast drying hydroxy acrylic resin of the present invention has an ultra-fast drying property. When added to the polyurethane varnish, the coating has excellent weather resistance, chemical corrosion resistance, hardness and decorative properties, and can meet the use requirements in various harsh environments.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] In a first aspect, the present invention provides a method for preparing an ultra-fast drying hydroxylated acrylic resin, comprising the following steps:

[0006] (1) 12-16 parts by weight of a high-activity hydroxyl monomer, 21-28 parts by weight of an acrylate monomer, 14-19 parts by weight of a methacrylic acid monomer, and 20-35 parts by weight of a solvent are uniformly mixed to obtain a premixed solution; the high-activity hydroxyl monomer comprises hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is (1-3):(1-2);

[0007] (2) adding 0.6-1.4 parts by weight of initiator, 0.7-1.2 parts by weight of chain transfer agent and 1-3 parts by weight of functional additive to the premixed solution, the reaction temperature is 140-160° C., and the reaction time is 2-3 hours;

[0008] (3) Then, the temperature is lowered to 60-70° C., 0.01-0.05 parts by weight of a catalyst is added, mixed evenly, and filtered to obtain an ultra-fast drying hydroxy acrylic resin.

[0009] The invention adopts hydroxyethyl acrylate and hydroxyethyl methacrylate as high-activity hydroxyl monomers, and compound them with acrylate monomers and methacrylic acid monomers, so as to increase the glass transition temperature of the resin, thereby improving the quick-drying property of the resin.

[0010] Preferably, the catalyst in step (3) comprises dibutyltin oxide and dibutyltin dilaurate, and the mass ratio of dibutyltin oxide to dibutyltin dilaurate is (1-4):1.

[0011] The invention adopts dibutyltin oxide and dibutyltin dilaurate in a specific ratio as catalysts, which can further accelerate the curing reaction of the resin, thereby improving the quick-drying property of the resin.

[0012] Preferably, the acrylic acid ester monomer in step (1) is at least one of butyl acrylate, ethyl acrylate and cyclohexyl acrylate.

[0013] Preferably, the methacrylic acid monomer in step (1) includes at least one of hydroxyethyl methacrylate and glycidyl methacrylate.

[0014] Preferably, the solvent in step (1) comprises at least one of butyl acetate, n-butanol and xylene.

[0015] Preferably, the functional auxiliary agent in step (2) includes a cross-linking agent, preferably a blocked isocyanate.

[0016] The invention can increase the cross-linking density of the resin by adding a cross-linking agent, which can not only improve the quick-drying property of the resin, but also improve the weather resistance of the resin.

[0017] Preferably, the functional additive in step (2) further includes a leveling agent.

[0018] Preferably, the initiator in step (2) includes at least one of azobisisobutyronitrile, tert-butyl peroxide, benzoyl peroxide, and tert-amyl peroxide.

[0019] Preferably, the chain transfer agent in step (2) is 3-mercapto-1-propanol.

[0020] In a second aspect, the present invention further provides an ultra-fast drying hydroxylated acrylic resin prepared by the above method, wherein the ultra-fast drying hydroxylated acrylic resin has a hydroxyl value of 80-100 KOH / g.

[0021] In a third aspect, the present invention further provides a polyurethane varnish, wherein component A comprises the following components by weight: 80 parts of super fast-drying hydroxy acrylic resin; 5-10 parts of pigment; 8-12 parts of filler; 6-15 parts of environmentally friendly additive; 10-30 parts of water;

[0022] Component B includes the following components: 18-35 parts of isocyanate curing agent.

[0023] The invention adopts super fast drying hydroxy acrylic resin and isocyanate curing agent for compounding, so that the prepared paint film has fast drying speed and high hardness, so that the polyurethane varnish coating film has excellent weather resistance, chemical corrosion resistance, hardness and decorativeness.

[0024] Preferably, the isocyanate curing agent includes toluene diisocyanate (TDI) and hexamethylene diisocyanate (HDI).

[0025] More preferably, the mass ratio of toluene diisocyanate (TDI) to hexamethylene diisocyanate (HDI) is 1:(1-2).

[0026] Preferably, the pigment includes at least one of red iron oxide, carbon black and titanium dioxide.

[0027] Preferably, the filler includes at least one of mica powder, silica powder, barium sulfate and silicon dioxide.

[0028] Preferably, the environmentally friendly additive includes at least one of a film-forming additive, a defoaming agent, a wetting agent, a pH regulator, and a dispersant.

[0029] More preferably, the film-forming aid is dipropylene glycol butyl ether; the defoaming agent is a silicone defoaming agent; the wetting agent is a polyether silicone copolymer; the pH adjuster includes at least one of ammonia water, N,N-dimethylethanolamine, and triethylamine; and the dispersant is a polyether acrylate polymer.

[0030] In a fourth aspect, the present invention further provides a method for preparing a polyurethane varnish, comprising the following steps:

[0031] (1) uniformly mixing the components in component A according to the proportions to obtain component A;

[0032] (2) During construction, mix component A and component B in a weight ratio of 1:(2-3).

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The ultra-fast drying hydroxy acrylic resin of the present invention has an ultra-fast drying property. When added to a polyurethane varnish, the coating has excellent weather resistance, chemical corrosion resistance, hardness and decorative properties, and can meet the use requirements in various harsh environments.

[0035] (2) The preparation method of the present invention is simple and convenient, has good environmental performance, is suitable for a variety of coating processes, and has broad application prospects. DETAILED DESCRIPTION

[0036] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the protection scope and implementation methods of the present invention are not limited thereto.

[0037] Unless otherwise specified, the materials and reagents used in the following examples are commercially available.

[0038] Example 1

[0039] This embodiment discloses a method for preparing an ultra-fast drying hydroxylated acrylic resin, comprising the following steps:

[0040] (1) 15 parts by weight of a highly active hydroxyl monomer, 24 parts by weight of an acrylate monomer, 16 parts by weight of a methacrylic acid monomer, and 30 parts by weight of a solvent were mixed uniformly to obtain a premixed solution;

[0041] The highly active hydroxy monomer includes hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 1:2; the acrylic acid ester monomer is butyl acrylate; the methacrylic acid monomer is glycidyl methacrylate; and the solvent is butyl acetate;

[0042] (2) Add 1.4 parts of initiator, 1.06 parts of chain transfer agent and 2 parts of functional additive to the premixed solution, the reaction temperature is 140°C, and the reaction time is 2.5 hours;

[0043] The initiator is azobisisobutyronitrile; the chain transfer agent is 3-mercapto-1-propanol; the functional additives include 1 part of a crosslinking agent and 1 part of a leveling agent, the crosslinking agent is a blocked isocyanate (JB-696C from Suzhou Jiubang Chemical), and the leveling agent is a polyurethane leveling rheological agent (BYK, BYK333);

[0044] (3) Then the temperature is lowered to 65° C., 0.04 parts of a catalyst is added, mixed evenly and filtered to obtain an ultra-fast drying hydroxy acrylic resin; the catalyst is dibutyltin oxide.

[0045] This embodiment also discloses a polyurethane varnish, wherein component A comprises the following components by weight: 80 parts of super fast-drying hydroxy acrylic resin; 5 parts of pigment; 8 parts of filler; 6 parts of environmentally friendly additive; 20 parts of water;

[0046] The pigment is carbon black; the filler is mica powder; the environmentally friendly additives include film-forming additives, defoaming agents, wetting agents, pH adjusters, and dispersants, and their mass ratio is 1:1:1:1:1:1. The film-forming additive is dipropylene glycol butyl ether, the defoaming agent is a silicone defoaming agent (TEGO ARIEX 902W, Evonik), the wetting agent is a polyether siloxy copolymer (WET 270), the pH adjuster includes ammonia water, and the dispersant is a polyether acrylate polymer (BYK, BYK190).

[0047] Component B includes the following components: 30 parts of an isocyanate curing agent, the isocyanate curing agent includes toluene diisocyanate (TDI) and hexamethylene diisocyanate (HDI), and the mass ratio of TDI:HDI is 1:2.

[0048] This embodiment also discloses a method for preparing a polyurethane varnish, comprising the following steps:

[0049] (1) uniformly mixing the components in component A according to the proportions to obtain component A;

[0050] (2) During construction, mix component A and component B in a weight ratio of 1:2.

[0051] Example 2

[0052] A method for preparing an ultra-fast drying hydroxylated acrylic resin, which is different from Example 1 only in that the highly active hydroxyl monomer in step (1) comprises hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 1:1.

[0053] Example 3

[0054] A method for preparing an ultra-fast drying hydroxylated acrylic resin, which is different from Example 1 only in that the high-activity hydroxyl monomer in step (1) comprises hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 3:2.

[0055] Example 4

[0056] A method for preparing an ultra-fast drying hydroxylated acrylic resin, which is different from Example 1 only in that the highly active hydroxyl monomer in step (1) comprises hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 3:1.

[0057] Example 5

[0058] A method for preparing an ultra-fast drying hydroxy acrylic resin, which is different from Example 1 only in that the catalyst in step (3) comprises dibutyltin oxide and dibutyltin dilaurate, and the mass ratio of dibutyltin oxide to dibutyltin dilaurate is 1:1.

[0059] Example 6

[0060] A method for preparing an ultra-fast drying hydroxy acrylic resin, which is different from Example 1 only in that the catalyst in step (3) includes dibutyltin oxide and dibutyltin dilaurate, and the mass ratio of dibutyltin oxide to dibutyltin dilaurate is 2:1.

[0061] Example 7

[0062] A method for preparing an ultra-fast drying hydroxy acrylic resin, which is different from Example 1 only in that the catalyst in step (3) includes dibutyltin oxide and dibutyltin dilaurate, and the mass ratio of dibutyltin oxide to dibutyltin dilaurate is 3:1.

[0063] Example 8

[0064] A method for preparing an ultra-fast drying hydroxy acrylic resin, which is different from Example 1 only in that the catalyst in step (3) includes dibutyltin oxide and dibutyltin dilaurate, and the mass ratio of dibutyltin oxide to dibutyltin dilaurate is 4:1.

[0065] Example 9

[0066] A method for preparing an ultra-fast drying hydroxy acrylic resin, which is different from Example 1 only in that the mass fractions of raw material components for preparing the ultra-fast drying hydroxy acrylic resin are different, comprises the following steps:

[0067] (1) By weight, 12 parts of a highly active hydroxyl monomer, 21 parts of an acrylate monomer, 14 parts of a methacrylic acid monomer, and 35 parts of a solvent were mixed uniformly to obtain a premixed solution;

[0068] The highly active hydroxy monomer includes hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 1:2; the acrylic acid ester monomer is butyl acrylate; the methacrylic acid monomer is glycidyl methacrylate; and the solvent is butyl acetate;

[0069] (2) Add 0.6 parts of initiator, 0.7 parts of chain transfer agent and 1 part of functional additive to the premixed solution, the reaction temperature is 140°C, and the reaction time is 2.5 hours;

[0070] The initiator is azobisisobutyronitrile; the chain transfer agent is 3-mercapto-1-propanol; the functional additives include 0.5 parts of a crosslinking agent and 0.5 parts of a leveling agent, the crosslinking agent is a blocked isocyanate (JB-696C from Suzhou Jiubang Chemical), and the leveling agent is a polyurethane leveling rheological agent (BYK, BYK333);

[0071] (3) Then the temperature is lowered to 65° C., 0.01 parts of a catalyst is added, mixed evenly and filtered to obtain an ultra-fast drying hydroxy acrylic resin; the catalyst is dibutyltin oxide.

[0072] Example 10

[0073] A method for preparing an ultra-fast drying hydroxy acrylic resin, which is different from Example 1 only in that the mass fractions of raw material components for preparing the ultra-fast drying hydroxy acrylic resin are different, comprises the following steps:

[0074] (1) By weight, 16 parts of a highly active hydroxyl monomer, 28 parts of an acrylate monomer, 19 parts of a methacrylic acid monomer, and 20 parts of a solvent were mixed uniformly to obtain a premixed solution;

[0075] The highly active hydroxy monomer includes hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 1:2; the acrylic acid ester monomer is butyl acrylate; the methacrylic acid monomer is glycidyl methacrylate; and the solvent is butyl acetate;

[0076] (2) Add 1.4 parts of initiator, 1.2 parts of chain transfer agent and 3 parts of functional additive to the premixed solution, the reaction temperature is 140°C, and the reaction time is 2.5 hours;

[0077] The initiator is azobisisobutyronitrile; the chain transfer agent is 3-mercapto-1-propanol; the functional additives include 1 part of a crosslinking agent and 2 parts of a leveling agent, the crosslinking agent is a blocked isocyanate (JB-696C from Suzhou Jiubang Chemical), and the leveling agent is a polyurethane leveling rheological agent (BYK, BYK333);

[0078] (3) Then the temperature is lowered to 65° C., 0.05 parts of a catalyst is added, mixed evenly and filtered to obtain an ultra-fast drying hydroxy acrylic resin; the catalyst is dibutyltin oxide.

[0079] Comparative Example 1

[0080] A method for preparing an ultra-fast-drying hydroxylated acrylic resin, which differs from Example 1 only in that the highly active hydroxyl monomer in step (1) is hydroxyethyl acrylate.

[0081] Comparative Example 2

[0082] A method for preparing an ultra-fast-drying hydroxylated acrylic resin, which differs from Example 1 only in that the highly active hydroxyl monomer in step (1) is ethyl hydroxyhexanoate.

[0083] Comparative Example 3

[0084] A method for preparing an ultra-fast drying hydroxylated acrylic resin, which is different from Example 1 only in that the high-activity hydroxyl monomer in step (1) comprises hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 1:3.

[0085] Comparative Example 4

[0086] A method for preparing an ultra-fast drying hydroxylated acrylic resin, which is different from Example 1 only in that the highly active hydroxyl monomer in step (1) comprises hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is 4:1.

[0087] Comparative Example 5

[0088] A method for preparing an ultra-fast-drying hydroxylated acrylic resin, which is different from Example 1 only in that no acrylic acid ester monomer is added in step (1).

[0089] Comparative Example 6

[0090] A method for preparing an ultra-fast-drying hydroxylated acrylic resin, which is different from Example 1 only in that no methacrylic acid monomer is added in step (1).

[0091] Comparative Example 7

[0092] A method for preparing an ultra-fast drying hydroxy acrylic resin, which is different from Example 1 only in that the reaction temperature in step (2) is 170°C.

[0093] Comparative Example 8

[0094] A method for preparing an ultra-fast-drying hydroxylated acrylic resin, which is different from Example 1 only in that the reaction time in step (2) is 1 hour.

[0095] In order to verify the performance of the ultra-fast drying hydroxy acrylic resin and polyurethane varnish of the present invention, the polyurethane varnish prepared in each embodiment and comparative example was sprayed on tinplate to obtain a pre-coated plate sample for performance evaluation test.

[0096] 1. Surface drying time / actual drying time: tested in accordance with GB / T1728-1979 standard.

[0097] 2. Hardness: Tested in accordance with GB / T6739-2006 standard. The higher the hardness grade, the greater the hardness.

[0098] 3. Gloss: Tested in accordance with GB / T9754-2007 standard.

[0099] 4. VOC: Tested in accordance with GB / T23985-2009 standard.

[0100] 5. Weather resistance: Tested in accordance with GB / T14522-2008 standard.

[0101] 6. Chemical corrosion resistance: (1) Acid resistance: Soak the pre-coated board sample in 0.05N sulfuric acid solution for 24 hours; (2) Alkali resistance: Soak the pre-coated board sample in 0.1N sodium hydroxide solution for 24 hours.

[0102] The above test results are shown in Table 1 and Table 2.

[0103] Table 1

[0104]

[0105]

[0106] Table 2

[0107]

[0108]

[0109] According to Table 3, the surface drying time of the coating film is 8-19 minutes, the actual drying time is 1.5-2.4 hours, the hardness grade is H, the gloss is more than 95%, and the VOC is less than 200 g / L, which shows that the polyurethane varnish of the present invention has excellent weather resistance, chemical corrosion resistance, hardness and decorativeness, can meet the use requirements in various harsh environments, and meets environmental protection requirements.

[0110] According to the comparison of Comparative Examples 1-6 with Example 1, it can be obtained that in Comparative Examples 1-2, the high-activity hydroxyl monomer is compounded with hydroxyethyl acrylate or hydroxyethyl acrylate and methacrylic acid monomers, and the surface-drying time and the actual drying time of the paint film are much longer than that of Example 1; in Comparative Example 3, no acrylate monomer is added, and in Comparative Example 4, no methacrylic acid monomer is added, and the surface-drying time and the actual drying time of the paint film are also longer than that of Example 1. In Example 1, the high-activity hydroxyl monomer is compounded with hydroxyethyl acrylate and hydroxyethyl acrylate and methacrylic acid monomers, and the surface-drying time and the actual drying time of the paint film are greatly shortened, indicating that only by compounding hydroxyethyl acrylate and hydroxyethyl acrylate and methacrylic acid monomers at the same time and coordinating with acrylate monomers and methacrylic acid monomers can the quick-drying property of the resin be better improved.

[0111] According to Examples 1-4, as the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate gradually increases, the surface drying time and the actual drying time of the paint film first decrease and then increase, indicating that the present invention can optimize the quick-drying performance of the resin by controlling the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate to (1-3): (1-2).

[0112] By comparing Examples 5-8 with Example 1, it can be seen that the catalysts in Examples 5-8 are compounded with dibutyltin oxide and dibutyltin dilaurate, and the mass ratio of dibutyltin oxide to dibutyltin dilaurate is controlled to (1-4):1, which can further improve the quick-drying property of the resin.

[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing an ultra-fast drying hydroxylated acrylic resin, characterized in that: The following steps are involved: (1) 12-16 parts by weight of a high-activity hydroxyl monomer, 21-28 parts by weight of an acrylate monomer, 14-19 parts by weight of a methacrylic acid monomer, and 20-35 parts by weight of a solvent are uniformly mixed to obtain a premixed solution; the high-activity hydroxyl monomer comprises hydroxyethyl acrylate and hydroxyethyl acrylate caproate, and the mass ratio of hydroxyethyl acrylate to hydroxyethyl acrylate caproate is (1-3):(1-2); (2) adding 0.6-1.4 parts by weight of initiator, 0.7-1.2 parts by weight of chain transfer agent and 1-3 parts by weight of functional additive to the premixed solution, the reaction temperature is 140-160° C., and the reaction time is 2-3 hours; (3) Then, the temperature is lowered to 60-70° C., 0.01-0.05 parts by weight of a catalyst is added, mixed evenly, and filtered to obtain an ultra-fast drying hydroxy acrylic resin.

2. The method for preparing the super fast-drying hydroxy acrylic resin according to claim 1, characterized in that: The catalyst in step (3) includes dibutyltin oxide and dibutyltin dilaurate.

3. The method for preparing the super fast-drying hydroxy acrylic resin according to claim 2, characterized in that: The mass ratio of dibutyltin oxide to dibutyltin dilaurate is (1-4):

1.

4. The method for preparing the ultra-fast drying hydroxy acrylic resin according to claim 1, characterized in that: The step (1) comprises at least one of (a) to (c): (a) the acrylic acid ester monomer is at least one of butyl acrylate, ethyl acrylate and cyclohexyl acrylate; (b) the methacrylic acid monomer comprises at least one of hydroxyethyl methacrylate and glycidyl methacrylate; (c) The solvent includes at least one of butyl acetate, n-butanol and xylene.

5. The method for preparing the super fast-drying hydroxy acrylic resin according to claim 1, characterized in that: The step (2) comprises at least one of (a) to (c): (a) The functional additives include a crosslinking agent and a leveling agent; (b) the initiator comprises at least one of azobisisobutyronitrile, tert-butyl peroxide, benzoyl peroxide, and tert-amyl peroxide; (c) The chain transfer agent is 3-mercapto-1-propanol.

6. The ultra-fast drying hydroxy acrylic resin prepared by the method according to any one of claims 1 to 5.

7. A polyurethane varnish, characterized in that: Component A comprises the following components in parts by mass: 80 parts of the super fast-drying hydroxy acrylic resin as claimed in claim 6; Pigment 5-10 parts; filler 8-12 parts; Environmentally friendly additives 6-15 parts; water 10-30 parts; Component B includes the following components: 18-35 parts of isocyanate curing agent.

8. The polyurethane varnish according to claim 7, characterized in that The isocyanate curing agent includes toluene diisocyanate and hexamethylene diisocyanate, and the mass ratio of the toluene diisocyanate to the hexamethylene diisocyanate is 1:(1-2).

9. The polyurethane varnish according to claim 7, characterized in that At least one of the following: The pigment includes at least one of red iron oxide, carbon black and titanium dioxide; The filler includes at least one of mica powder, silicon powder, barium sulfate and silicon dioxide; The environmentally friendly additive includes at least one of a film-forming additive, a defoaming agent, a wetting agent, a pH regulator, and a dispersant.

10. The method for preparing the polyurethane varnish according to any one of claims 7 to 9, characterized in that: The following steps are involved: (1) uniformly mixing the components in component A according to the proportions to obtain component A; (2) During construction, mix component A and component B in a weight ratio of 1:(2-3).