Hydrogel lens and preparation method thereof
By introducing trimethylsiloxane, amide and carboxylic structures into hydrogel lenses, the oxygen permeability and toughness are improved, the problem of low oxygen permeability of traditional hydrogel corneal contact lenses is solved, and the use of lenses is extended Lifespan and improve wear comfort.
Patent Information
- Application Number
- CN202411255768.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-12
AI Technical Summary
The oxygen permeability of traditional hydrogel corneal contact lenses is low, resulting in corneal hypoxia during long-term wear, which in turn causes ocular surface problems such as dry eye, conjunctival congestion and corneal edema.
The polymer of hydrogel lenses is introduced into trimethylsiloxane, amide and carboxylic structures, and the combination of hydroxy methacrylate monomers, N-hydroxyethyl acrylamide and small molecule silicon monomers, Improve the oxygen permeability, toughness and moisture content of the lens, reduce the elastic modulus, and enhance the comfort of wearing.
It significantly improves the oxygen permeability of hydrogel lenses, extends the life cycle of the lenses, reduces the breaking rate, improves the comfort of wearing, and ensures compatibility of the preparation raw materials by adjusting the types and content of small-molecular silicon monomers. and no solvent addition required.
Smart Images

Figure BDA0005035283130000011 
Figure BDA0005035283130000051 
Figure FDA0005035283120000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of contact lenses, and in particular to a hydrogel lens and a preparation method thereof. Background Art
[0002] Contact lenses, also known as corneal contact lenses, can be used to correct vision, protect the eyeballs or increase the beauty of the eyes, and are therefore very popular among people.
[0003] With the development of science and technology, corneal contact lenses have gradually evolved from early hard materials to soft materials with better comfort. Soft corneal contact lenses, also known as hydrogel corneal contact lenses, have good chemical stability, biocompatibility, ion permeability, surface wettability, mechanical properties and other characteristics. Traditional hydrogel corneal contact lenses are made of hydrophilic monomers and generally have low oxygen permeability. Long-term wearing can cause corneal hypoxia, leading to ocular surface problems such as dry eyes, conjunctival congestion, and corneal edema. Summary of the invention
[0004] The invention provides a hydrogel lens and a preparation method thereof. The hydrogel lens of the invention has high oxygen permeability.
[0005] The present invention provides a hydrogel lens, wherein the polymer in the hydrogel lens contains trimethylsiloxane, amide group and carboxyl group;
[0006] The polymer is obtained by polymerizing hydroxy methacrylate monomers, N-hydroxyethyl acrylamide and a small molecule silicon monomer containing trimethylsiloxane.
[0007] Preferably, the following raw materials are included in the preparation, by weight:
[0008]
[0009] Preferably, the hydroxy methacrylate monomers include hydroxyalkyl methacrylate and / or glycerol methacrylate.
[0010] Preferably, the hydroxyalkyl methacrylate includes one or more of hydroxyethyl methacrylate, hydroxybutyl methacrylate and hydroxypropyl methacrylate.
[0011] Preferably, the small molecule silicon monomer includes one or more of methacryloxypropyl tris(trimethylsiloxane)silane, (3-methacrylamidepropyl)bis(trimethylsiloxane)methylsilane, acrylamidopropyl tris(trimethylsiloxane)silane, 3-(methacryloxy)propyl trimethoxysilane, methacryloxymethyl tris(trimethylsiloxy)silane and methacrylamidopropyl bis(trimethylsiloxane)silanol and 3-(3-methacryloxy-2-hydroxypropyl)propyl bis(trimethylsiloxane)methylsilane.
[0012] Preferably, the crosslinking agent includes one or more of triethylene glycol diacrylate, triallyl isocyanurate, triethylene glycol dimethacrylate, triethylene glycol divinyl ester, vinyl methacrylate, divinyl glycol, polyethylene glycol dimethacrylate and divinyl polyethylene glycol ester.
[0013] Preferably, the initiator comprises a thermal initiator.
[0014] Preferably, the thermal initiator includes one or more of azobisisobutyronitrile, azobisisoheptanenitrile and peroxide.
[0015] Preferably, the peroxide comprises one or more of benzoyl peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate and bis(2-phenylethoxy) peroxydicarbonate.
[0016] The present invention also provides a method for preparing the hydrogel lens described in the above technical solution, comprising the following steps:
[0017] The raw materials for preparing the hydrogel lens are mixed and then injected into a mold for polymerization reaction, and the obtained polymerization reaction product is demolded and then immersed in water for hydration to obtain the hydrogel lens.
[0018] The present invention provides a hydrogel lens, wherein the polymer in the hydrogel lens contains methylsiloxane, amide group and carboxyl group;
[0019] The polymer is obtained by polymerizing hydroxy methacrylate monomers, N-hydroxyethyl acrylamide and a small molecule silicon monomer containing methylsiloxane.
[0020] The present invention improves the hydrophilicity and water content of the hydrogel lens by adding hydrophilic groups (amide and carboxyl) to the polymer of the hydrogel lens, and improves the oxygen permeability of the hydrogel lens by combining the trimethylsiloxane structure introduced into the polymer (the trimethylsiloxane structure has a weak polarity, the chain segments are easy to rotate, and oxygen is easy to penetrate through the trimethylsiloxane structure). The results of the embodiment show that the oxygen permeability of the hydrogel lens of the present invention is 33.21×10 -11 ~47.8×10 -11 (cm 2 / s)[mLO2 / (mL)·mmhg.
[0021] The present invention improves the toughness of the hydrogel lens by compounding hydroxy methacrylate monomers, N-hydroxyethyl acrylamide and small molecule silicon monomers, thereby increasing the life cycle of the hydrogel lens and reducing the breakage rate of the hydrogel lens during use; in addition, the N-hydroxyethyl acrylamide containing amide groups and carboxyl groups increases the water content of the hydrogel lens, thereby reducing the elastic modulus of the lens and improving the wearing comfort of the hydrogel lens.
[0022] Furthermore, the present invention adjusts the type and content of the small molecule silicon monomer so that no solvent needs to be added to prepare the raw materials and the compatibility of the raw materials is good. DETAILED DESCRIPTION
[0023] The present invention provides a hydrogel lens, wherein the polymer in the hydrogel lens contains methylsiloxane, amide group and carboxyl group;
[0024] The polymer is obtained by polymerizing hydroxy methacrylate monomers, N-hydroxyethyl acrylamide and a small molecule silicon monomer containing methylsiloxane.
[0025] In the present invention, the water content of the hydrogel lens is preferably 50-70 wt %, more preferably 51.3-67.44 wt %, and further preferably 55.21-60 wt %.
[0026] In the present invention, the raw materials for preparing the hydrogel lens include 40 to 70 parts by mass, preferably 45 to 60 parts, and more preferably 50 to 55 parts of hydroxyl methacrylate monomers; the hydroxyl methacrylate monomers preferably include hydroxyalkyl methacrylate and / or glyceryl methacrylate; the hydroxyalkyl methacrylate preferably includes one or more of hydroxyethyl methacrylate, hydroxybutyl methacrylate and hydroxypropyl methacrylate.
[0027] Based on the mass fraction of the hydroxy methacrylate monomer, the raw material for preparing the hydrogel lens includes 30 to 40 parts of N-hydroxyethyl acrylamide, preferably 35 to 36 parts.
[0028] Based on the mass fraction of the hydroxy methacrylate monomer, the raw materials for preparing the hydrogel lens include 5 to 20 parts of small molecule silicon monomers, preferably 10 to 18 parts, and more preferably 12 to 15 parts; the small molecule silicon monomers preferably include one or more of methacryloxypropyl tris(trimethylsiloxy)silane, (3-methacrylamidepropyl)bis(trimethylsiloxane)methylsilane, acrylamidopropyl tris(trimethylsiloxane)silane, 3-(methacryloxy)propyl trimethoxysilane, methacryloxymethyl tris(trimethylsiloxy)silane, methacrylamidopropyl bis(trimethylsiloxane)silanol and 3-(3-methacryloxy-2-hydroxypropyl)propyl bis(trimethylsiloxane)methylsilane.
[0029] Based on the mass fraction of the hydroxy methacrylate monomer, the raw materials for preparing the hydrogel lens include 0.0075 to 3.9 parts of a cross-linking agent, preferably 1 to 3 parts, and more preferably 1.5 to 2 parts; the cross-linking agent preferably includes one or more of triethylene glycol diacrylate, triallyl isocyanurate, triethylene glycol dimethacrylate, triethylene glycol divinyl ester, vinyl methacrylate, divinyl glycol ester, polyethylene glycol dimethacrylate, and divinyl polyethylene glycol ester.
[0030] Based on the mass fraction of the hydroxy methacrylate monomer, the raw materials for preparing the hydrogel lens include 0.0075 to 3.9 parts of an initiator, preferably 1 to 3 parts, and more preferably 1.5 to 2 parts; the initiator preferably includes a thermal initiator; the thermal initiator preferably includes one or more of azobisisobutyronitrile, azobisisoheptanenitrile and peroxide; the peroxide preferably includes one or more of benzoyl peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate and bis(2-phenylethoxy) peroxydicarbonate.
[0031] The present invention also provides a method for preparing the hydrogel lens described in the above technical solution, comprising the following steps:
[0032] The raw materials for preparing the hydrogel lens are mixed and then injected into a mold for polymerization reaction, and the obtained polymerization reaction product is demolded and then immersed in water for hydration to obtain the hydrogel lens.
[0033] In the present invention, the mixing is preferably carried out under the condition of magnetic stirring, and the mixing time is preferably 12 hours.
[0034] In the present invention, the polymerization reaction temperature is preferably 50 to 120° C., more preferably 80 to 100° C., and the polymerization reaction time is preferably 5 to 20 hours, more preferably 8 to 10 hours.
[0035] After the hydration, the present invention preferably further comprises: performing solid-liquid separation on the mixture obtained by hydration, and then immersing the obtained lens in physiological saline for equilibrium to obtain the hydrogel lens.
[0036] After the hydration, water enters the polymer obtained by the polymerization reaction, generating a water-containing contact lens.
[0037] The hydrogel lens and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0038] Example 1
[0039] Weigh 50 parts of hydroxyethyl methacrylate (HEMA), 10 parts of 3-(3-methacryloyloxy-2-hydroxypropyl)propylbis(trimethylsiloxane)methylsilane (SIGMA), 40 parts of N-hydroxyethyl acrylamide (HEEA), 0.2 parts of ethylene glycol dimethacrylate (EGDMA), and 0.225 parts of azobisisobutyronitrile (AIBN) respectively, stir them magnetically for 12 hours, mix them evenly, add them dropwise to a corneal contact lens mold, cure them at 80°C for 24 hours, then demold, extract and remove unpolymerized monomers in the lens with deionized water, and after solid-liquid separation, immerse the obtained lens in physiological saline for equilibrium to obtain a corneal contact lens.
[0040] Example 2
[0041] Weigh 50 parts of hydroxyethyl methacrylate (HEMA), 20 parts of methacryloyloxypropyl tris(trimethylsiloxy)silane (Tris), 30 parts of N-hydroxyethyl acrylamide (HEEA), 0.2 parts of ethylene glycol dimethacrylate (EGDMA), and 0.225 parts of azobisisobutyronitrile (AIBN) respectively, stir them magnetically for 12 hours, mix them evenly, add them dropwise to a corneal contact lens mold, cure them at 120°C for 8 hours, then demold, extract and remove unpolymerized monomers in the lens with deionized water, and after solid-liquid separation, immerse the obtained lens in physiological saline for equilibrium to obtain a corneal contact lens.
[0042] Example 3
[0043] Weigh 55 parts of hydroxypropyl methacrylate (HPMA), 15 parts of 3-(3-methacryloyloxy-2-hydroxypropyl)propylbis(trimethylsiloxane)methylsilane (SIGMA), 30 parts of N-hydroxyethyl acrylamide (HEEA), 0.2 parts of triethylene glycol dimethacrylate (TEGDMA), and 0.225 parts of azobisisobutyronitrile (AIBN) respectively, stir them magnetically for 12 hours, mix them evenly, add them dropwise to a corneal contact lens mold, cure them at 90°C for 12 hours, then demold, extract and remove unpolymerized monomers in the lens with deionized water, and after solid-liquid separation, immerse the obtained lens in physiological saline for equilibrium to obtain a corneal contact lens.
[0044] Examples 4 to 6, Comparative Examples 1 to 3
[0045] The preparation methods of Examples 4 to 6 and Comparative Examples 1 to 3 are the same as those of Example 1, except for the raw materials. The raw materials for the preparation of Examples 4 to 6 and Comparative Examples 1 to 3 are shown in Table 1.
[0046] The oxygen permeability values of the corneal contact lenses prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were measured respectively by polarography according to the national standard (GBT 11417.3-2012). The test results are listed in Table 1.
[0047] The moisture content of the corneal contact lenses prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was measured by weighing method. The weight of the glass slide was Q1, the weight of the lens and the glass slide was Q2, and after drying in an oven at 105° C. to constant weight, the gross weight was G3. The moisture content = (Q2-G3) / (Q2-Q1). The test results are listed in Table 1.
[0048] The elongation of the corneal contact lenses of Examples 1 to 3 and Comparative Examples 1 to 3 was tested using an electronic tensile testing machine XLW (PC). Each sample was clamped with a clamp for measurement, and the elongation at break of the corneal contact lens samples was measured. The test results are listed in Table 1.
[0049] Table 1 Preparation materials and test results of corneal contact lenses of Examples 1 to 3 and Comparative Examples 1 to 3
[0050]
[0051] As can be seen from Table 1, the elongation of the lens prepared by the present invention reaches more than 300%, has strong toughness, oxygen permeability is 3 to 4 times that of ordinary hydrogels, and has a very high water content of more than 50%.
[0052] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A hydrogel lens, characterized in that: The polymer in the hydrogel lens contains trimethylsiloxane, amide groups and carboxyl groups; The polymer is obtained by polymerizing hydroxy methacrylate monomers, N-hydroxyethyl acrylamide and a small molecule silicon monomer containing trimethylsiloxane.
2. The hydrogel lens according to claim 1, characterized in that: The preparation includes the following raw materials by weight:
3. The hydrogel lens according to claim 2, characterized in that: The hydroxy methacrylate monomers include hydroxyalkyl methacrylate and / or glyceryl methacrylate.
4. The hydrogel lens according to claim 3, characterized in that: The hydroxyalkyl methacrylate includes one or more of hydroxyethyl methacrylate, hydroxybutyl methacrylate and hydroxypropyl methacrylate.
5. The hydrogel lens according to claim 2, characterized in that: The small molecule silicon monomer includes one or more of methacryloxypropyl tris(trimethylsiloxy)silane, (3-methacrylamidepropyl)bis(trimethylsiloxane)methylsilane, acrylamidopropyl tris(trimethylsiloxane)silane, 3-(methacryloxy)propyl trimethoxysilane, methacryloxymethyl tris(trimethylsiloxy)silane, methacrylamidopropyl bis(trimethylsiloxane)silanol and 3-(3-methacryloxy-2-hydroxypropyl)propyl bis(trimethylsiloxane)methylsilane.
6. The hydrogel lens according to claim 2, characterized in that: The crosslinking agent includes one or more of triethylene glycol diacrylate, triallyl isocyanurate, triethylene glycol dimethacrylate, triethylene glycol divinyl ester, vinyl methacrylate, divinyl glycol, polyethylene glycol dimethacrylate and divinyl polyethylene glycol ester.
7. The hydrogel lens according to claim 2, characterized in that: The initiator includes a thermal initiator.
8. The hydrogel lens according to claim 7, characterized in that: The thermal initiator includes one or more of azobisisobutyronitrile, azobisisoheptanenitrile and peroxide.
9. The hydrogel lens according to claim 8, characterized in that: The peroxide includes one or more of benzoyl peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate and bis(2-phenylethoxy) peroxydicarbonate.
10. The method for preparing a hydrogel lens according to any one of claims 1 to 9, characterized in that: The following steps are involved: The raw materials for preparing the hydrogel lens are mixed and then injected into a mold for polymerization reaction, and the obtained polymerization reaction product is demolded and then immersed in water for hydration to obtain the hydrogel lens.
Citation Information
Cited By