Polyurethane composite material applied to electronic cotton and preparation process of polyurethane composite material

Through the combination of modified isocyanate and hexagonal boron nitride-cellulose intercalation materials, the lack of mechanical properties of polyurethane electronic sponges in high stress and high wear scenarios is solved, the toughness and thermal stability of the material are improved, and the use is extended Lifespan and improve biocompatibility.

CN118930809APending Publication Date: 2024-11-12JIANGSU HENGGUANG NEW MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411045617.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Polyurethane electronic sponge has insufficient mechanical properties, is prone to damage in high stress and high wear scenarios, and has poor biocompatibility and thermal stability, which limits its wider application and performance improvement.

Method used

Using a combination of modified isocyanate and hexagonal boron nitride-cellulose intercalation materials, a multi-layer structure is formed through ultrasonic treatment, which enhances the toughness and thermal stability of the material, and forms hydrogen bonds in the polyurethane matrix to improve interface binding force and form three-dimensional Network structure to improve heat resistance.

Benefits of technology

It significantly improves the toughness and thermal stability of polyurethane materials, extends service life, enhances the tolerance to ultraviolet rays, avoids yellowing and aging, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004973409210000101
    Figure BDA0004973409210000101
  • Figure BDA0004973409210000111
    Figure BDA0004973409210000111
  • Figure BDA0004973409210000112
    Figure BDA0004973409210000112
Patent Text Reader

Abstract

The invention relates to the technical field of polyurethane materials, in particular to a polyurethane composite material applied to electronic cotton and a preparation process thereof.The polyurethane composite material comprises a component A and a component B. The component A is prepared from, by weight, 90-100 parts of modified isocyanate, 1-5 parts of silicone oil and 0.002-0.006 part of flame retardant; the component B is prepared from the following components in parts by weight: 120 to 150 parts of polyether polyol, 30 to 50 parts of intercalation material dispersion liquid, 0.5 to 0.8 part of diluent, 0.5 to 5 parts of catalyst and 0.1 to 3 parts of color paste. Through interaction of all the components, formation of a multi-layer cross-linked structure of the material is promoted, the cross-linking density and stability of a polyurethane matrix are improved, and then the physical performance, heat resistance and aging resistance of the composite material are improved; and it can be ensured that polyurethane prepared from MDI as a raw material does not have aging phenomena such as yellowing in the high-strength use process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane materials, and in particular to a polyurethane composite material used for electronic sponges and a preparation process thereof. Background Art

[0002] Polyurethane (PU) is a type of polymer material containing repeated -HNCO-O- groups on the main chain. Its basic chemical structure is a carbamate chain segment generated by the reaction of polyisocyanates and polyols. Polyurethane electronic sponges usually use polyether polyols as raw materials. Due to the large number of ether bonds in its molecular structure, the material has excellent flexibility and low-temperature performance. The content of isocyanate groups in polyisocyanates also has a significant effect on the properties of foam plastics. Polyurethane electronic sponges have a low density, but have extremely high elasticity and recovery ability. They can quickly return to their original state after being compressed, making them an ideal choice for packaging electronic components and integrated circuits. At the same time, the porous structure of polyurethane foam gives it a good energy absorption effect. When subjected to external impact and vibration, the foam can absorb energy through the deformation of the internal structure, thereby protecting the internal electronic components. Therefore, polyurethane electronic sponges are widely used in many fields such as electronics, automobiles, and aerospace. In the electronics industry, polyurethane electronic sponges are mainly used for packaging electronic components, integrated circuits, and precision instruments. In addition, polyurethane electronic sponges are also used to produce electromagnetic shielding materials to protect electronic equipment from electromagnetic interference. The application of polyurethane electronic sponge in the automotive industry is mainly reflected in seats, headrests, dashboards and other parts. Its high elasticity and energy absorption performance can improve riding comfort and safety, absorb the energy generated during collision, and reduce damage to passengers.

[0003] In the prior art, the mechanical properties of polyurethane electronic sponges are insufficient, especially in high-stress and high-wear application scenarios, which can cause the material to be easily damaged during use, affecting its service life. At the same time, polyurethane prepared with diphenylmethane diisocyanate (MDI) as raw material has good biocompatibility, but during long-term use, the material will age, such as yellowing, hardening, embrittlement, etc., and should not be exposed to light for a long time. In addition, the relatively poor thermal stability, relatively low electrical conductivity, and poor biocompatibility of polyurethane materials have limited their wider application and further improvement of performance to a certain extent. Summary of the invention

[0004] In order to solve the problems mentioned in the above background technology, the present invention provides a polyurethane composite material for electronic cotton and a preparation process thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A polyurethane composite material for electronic cotton comprises a component A and a component B, wherein the component A comprises, by weight, 90-100 parts of modified isocyanate, 1-5 parts of silicone oil and 0.002-0.006 parts of flame retardant, and the component B comprises, by weight, 120-150 parts of polyether polyol, 30-50 parts of intercalation material dispersion, 0.5-0.8 parts of diluent, 0.5-5 parts of catalyst and 0.1-3 parts of color paste.

[0007] The diluent includes one or more of propylene glycol methyl ether, triethylene glycol, ethylene glycol, dipropylene glycol, glycerol and water.

[0008] The polyether polyol includes one or more of polypropylene glycol, polyethylene glycol, and polytetramethylene glycol.

[0009] Furthermore, the intercalation material dispersion liquid is prepared by the following steps:

[0010] Hexagonal boron nitride and cellulose are added into ethanol, ultrasonically treated, a silane coupling agent is added, and the temperature is controlled to react to obtain an intercalation material dispersion.

[0011] Furthermore, the modified isocyanate is prepared by the following steps:

[0012] Add boron phosphide powder to diphenylmethane diisocyanate, stir at 80-90°C at a stirring speed of 300-400 rpm for 30-60 minutes, then add glutaraldehyde, and continue stirring at the same speed for 5-15 minutes to obtain modified isocyanate.

[0013] Furthermore, the mass ratio of the hexagonal boron nitride, cellulose, ethanol and silane coupling agent is (0.8-1.8): (0.5-1.5): (10-20): (0.04-0.08).

[0014] Furthermore, the frequency of the ultrasonic treatment is 20-30kHz, the power is 100-200W, the time of the ultrasonic treatment is 10-30min, the reaction temperature is 60-70°C, and the reaction time is 2-4h.

[0015] Further, the catalyst includes one or more of bis(dimethylaminoethyl)ether, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl)ether, triethylamine, triethylenediamine and N-methyldiethanolamine.

[0016] Furthermore, the mass ratio of the diphenylmethane diisocyanate, boron phosphide powder and glutaraldehyde is (120-150):(8-12):(1-3).

[0017] Furthermore, the diluent includes one or more of propylene glycol methyl ether, triethylene glycol, ethylene glycol, dipropylene glycol, glycerol and water; the polyether polyol includes one or more of polypropylene glycol, polyethylene glycol and polytetramethylene glycol; and the flame retardant is aluminum hydroxide or magnesium hydroxide.

[0018] According to another aspect of the present invention, a process for preparing the above-mentioned composite material is provided, comprising the following steps:

[0019] Component A: Add modified isocyanate, silicone oil and flame retardant into a mixer and stir for the first time at a stirring speed of 1000-1200 rpm for 10-20 min to obtain a mixture of component A;

[0020] Component B: Add polyether polyol, intercalation material dispersion, diluent, catalyst and color paste into the mixer, stir for the second time at a speed of 2000-2500rpm for 30-60s, and keep warm at 70-80℃ for 2-3h to obtain a mixture of component B.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. In the technical solution of the present invention, the dispersion of hexagonal boron nitride (h-BN) and cellulose in ethanol is a solid-liquid dispersion process. Ultrasonic treatment produces a high temperature and high pressure environment locally through the cavitation of sound waves, which helps to break the cohesion between solid particles and obtain h-BN-cellulose intercalation, showing multi-level and multi-scale characteristics. In the polyurethane matrix, the h-BN-cellulose intercalation forms a structure similar to a "brick wall", which helps to disperse and absorb energy through interlayer slip and rotation when the material is subjected to external forces, thereby effectively hindering the expansion of cracks. At the same time, the hydroxyl groups on the cellulose molecular chain can form hydrogen bonds with the polyurethane matrix and play the role of a "bridge", connecting cellulose and polyurethane matrix, improving the interfacial bonding force, and enabling the composite material to dissipate energy by breaking and reforming hydrogen bonds when subjected to external forces, while retaining the lightweight of the material and further enhancing the toughness of the material.

[0023] 2. During the preparation of modified isocyanate, the isocyanate group in the MDI molecule reacts with a small amount of glutaraldehyde to form a cross-linked structure. At the same time, the unsaturated boron atoms or phosphorus atoms on the surface of the boron phosphide powder contain lone pairs of electrons or empty orbitals, which form coordination bonds or covalent bonds with the isocyanate groups in the MDI molecules and the aldehyde groups of glutaraldehyde, so that the boron phosphide is anchored in the network structure, providing additional cross-linking points for the polyurethane molecular chain, forming a three-dimensional network structure. The three-dimensional network structure helps to improve the stability and heat resistance of the polyurethane matrix. It can ensure that the polyurethane prepared with MDI as the raw material will not suffer from aging phenomena such as yellowing during high-intensity use. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Unless otherwise specified, the raw materials used in the present invention are all from conventional products purchased from the market, wherein the silicone oil is dimethyl silicone oil (DC-200), and the color paste is yellow color paste, model BASF Paliotol Yellow L0960HD.

[0026] Preparation Example 1

[0027] The modified isocyanate is prepared by the following steps:

[0028] 80 g of boron phosphide powder was added to 1200 g of diphenylmethane diisocyanate, and stirred at 80° C. and 300 rpm for 30 min. Then 10 g of glutaraldehyde was added and stirred at the same speed for 5 min to obtain modified isocyanate.

[0029] The intercalation material dispersion is prepared by the following steps:

[0030] 80 g of hexagonal boron nitride and 50 g of cellulose were added to 1000 g of ethanol, and ultrasonic treatment was performed at a frequency of 20 kHz and a power of 100 W for 10 min. 4 g of silane coupling agent G-570 was added and reacted at 60° C. for 2 h to obtain an intercalation material dispersion.

[0031] Preparation Example 2

[0032] The modified isocyanate is prepared by the following steps:

[0033] 100 g of boron phosphide powder was added to 1350 g of diphenylmethane diisocyanate, and stirred at 85° C. and 350 rpm for 45 min. Then 20 g of glutaraldehyde was added and stirred at the same speed for 10 min to obtain modified isocyanate.

[0034] The intercalation material dispersion is prepared by the following steps:

[0035] 100 g of hexagonal boron nitride and 80 g of cellulose were added to 1500 g of ethanol, and ultrasonic treatment was performed at a frequency of 25 kHz and a power of 150 W for 10 min. 5 g of silane coupling agent G-570 was added and reacted at 65° C. for 2 h to obtain an intercalation material dispersion.

[0036] Preparation Example 3

[0037] The modified isocyanate is prepared by the following steps:

[0038] 120 g of boron phosphide powder was added to 1500 g of diphenylmethane diisocyanate, and stirred at 90° C. and 400 rpm for 60 min. Then 30 g of glutaraldehyde was added and stirred at the same speed for 15 min to obtain modified isocyanate.

[0039] The intercalation material dispersion is prepared by the following steps:

[0040] 180g hexagonal boron nitride and 150g cellulose were added to 2000g ethanol, and ultrasonic treatment was performed at a frequency of 30kHz and a power of 200W for 30min. 8g silane coupling agent G-570 was added and reacted at 70℃ for 4h to obtain an intercalation material dispersion.

[0041] Example 1

[0042] A preparation process for polyurethane composite materials for electronic sponges comprises the following steps:

[0043] Component A: Add 90 parts of the modified isocyanate prepared in Preparation Example 1, 1 part of silicone oil and 0.002 parts of aluminum hydroxide into a mixer, and stir for the first time at a speed of 1000 rpm for 10 minutes to obtain a component A mixture;

[0044] Component B: 120 parts of polypropylene glycol, 0.5 parts of propylene glycol methyl ether, 0.5 parts of bis(dimethylamino)ethyl ether (BDMAEE), 30 parts of the intercalation material dispersion prepared in Preparation Example 1 and 0.1 parts of color paste were weighed by weight and added into a mixer. The mixture was stirred for the second time at a stirring speed of 2000 rpm for 30 seconds and kept warm at 70°C for 2 hours to obtain a mixture of component B.

[0045] When used, the polyurethane electronic sponge comprises the following steps for preparation:

[0046] Add the B component mixture to the A component mixture, add 0.2 parts of the foaming agent hexane, stir for a second time at 2000 rpm for 5 minutes, pour the foamed material into the mold, and cure at 100°C for 2 hours to ensure that the material is completely cured and formed to obtain the electronic cotton polyurethane.

[0047] Example 2

[0048] A preparation process for polyurethane composite materials for electronic sponges comprises the following steps:

[0049] Component A: Add 92 parts of the modified isocyanate prepared in Preparation Example 2, 1.5 parts of silicone oil and 0.003 parts of magnesium hydroxide into a mixer, and stir for the first time at a speed of 1000 rpm for 10 minutes to obtain a component A mixture;

[0050] Component B: 130 parts of polyethylene glycol, 0.5 parts of triethylene glycol, 1 part of N,N-dimethylcyclohexylamine, 35 parts of the intercalation material dispersion prepared in Preparation Example 2 and 0.3 parts of color paste were weighed by weight and added into a mixer. Stir for the second time at a stirring speed of 2000 rpm for 35 seconds and keep warm at 70°C for 2 hours to obtain a mixture of component B.

[0051] When used, the polyurethane electronic sponge comprises the following steps for preparation:

[0052] Add the B component mixture to the A component mixture, add 0.2 parts of the foaming agent sodium bicarbonate, stir for a second time at 2000 rpm for 5 minutes, pour the foamed material into the mold, and cure at 100°C for 2 hours to ensure that the material is completely cured and formed to obtain the electronic cotton polyurethane.

[0053] Example 3

[0054] A preparation process for polyurethane composite materials for electronic sponges comprises the following steps:

[0055] Component A: Add 94 parts of the modified isocyanate prepared in Preparation Example 3, 2 parts of silicone oil and 0.003 parts of magnesium hydroxide into a mixer, and stir for the first time at a speed of 1100 rpm for 15 minutes to obtain a component A mixture;

[0056] Component B: 135 parts of polypropylene glycol, 0.7 parts of water, 2 parts of bis(dimethylaminoethyl) ether (BDMAEE), 38 parts of the intercalation material dispersion prepared in Preparation Example 3 and 1 part of color paste were weighed and added into a mixer. Stir for the second time at a stirring speed of 2000 rpm for 35 seconds and keep warm at 70°C for 2 hours to obtain a mixture of component B.

[0057] When used, the polyurethane electronic sponge comprises the following steps for preparation:

[0058] Add the B component mixture to the A component mixture, add 0.2 parts of the foaming agent hexane, stir for a second time at 2000 rpm for 5 minutes, pour the foamed material into the mold, and cure at 100°C for 2 hours to ensure that the material is completely cured and formed to obtain the electronic cotton polyurethane.

[0059] Example 4

[0060] A preparation process for polyurethane composite materials for electronic sponges comprises the following steps:

[0061] Component A: Add 95 parts of the modified isocyanate prepared in Preparation Example 1, 2.5 parts of silicone oil and 0.004 parts of magnesium hydroxide into a mixer, and stir for the first time at a speed of 1100 rpm for 15 minutes to obtain a component A mixture;

[0062] Component B: 135 parts of polypropylene glycol, 0.7 parts of water, 2 parts of bis(2-dimethylaminoethyl) ether, 40 parts of the intercalation material dispersion prepared in Preparation Example 1 and 1.5 parts of color paste were weighed and added into a mixer. Stir for the second time at a stirring speed of 2000 rpm for 35 seconds and keep warm at 70°C for 2 hours to obtain a mixture of component B.

[0063] When used, the polyurethane electronic sponge comprises the following steps for preparation:

[0064] Add the B component mixture to the A component mixture, add 0.2 parts of the foaming agent hexane, stir for a second time at 2000 rpm for 5 minutes, pour the foamed material into the mold, and cure at 100°C for 2 hours to ensure that the material is completely cured and formed to obtain the electronic cotton polyurethane.

[0065] Example 5

[0066] A preparation process for polyurethane composite materials for electronic sponges comprises the following steps:

[0067] Component A: Add 98 parts of the modified isocyanate prepared in Preparation Example 2, 2.5 parts of silicone oil and 0.005 parts of magnesium hydroxide into a mixer, and stir for the first time at a speed of 1200 rpm for 20 minutes to obtain a component A mixture;

[0068] Component B: 135 parts of polypropylene glycol, 0.7 parts of water, 3 parts of bis(dimethylaminoethyl) ether (BDMAEE), 45 parts of the intercalation material dispersion prepared in Preparation Example 2 and 1.5 parts of color paste were weighed and added into a mixer. Stir for the second time at a stirring speed of 2000 rpm for 50 seconds and keep warm at 75°C for 2.5 hours to obtain a mixture of component B.

[0069] When used, the polyurethane electronic sponge comprises the following steps for preparation:

[0070] Add the B component mixture to the A component mixture, add 0.2 parts of the foaming agent hexane, stir for a second time at 2000 rpm for 5 minutes, pour the foamed material into the mold, and cure at 100°C for 2 hours to ensure that the material is completely cured and formed to obtain the electronic cotton polyurethane.

[0071] Example 6

[0072] A preparation process for polyurethane composite materials for electronic sponges comprises the following steps:

[0073] Component A: Add 100 parts of the modified isocyanate prepared in Preparation Example 3, 5 parts of silicone oil and 0.006 parts of magnesium hydroxide into a mixer, and stir for the first time at a speed of 1200 rpm for 20 minutes to obtain a component A mixture;

[0074] Component B: 150 parts of polytetrahydrofuran diol, 0.8 parts of water, 5 parts of N-methyldiethanolamine, 50 parts of the intercalation material dispersion prepared in Preparation Example 3 and 3 parts of color paste are added to a mixer and stirred for the second time at a stirring speed of 2500 rpm for 60 seconds. The mixture is kept at 80°C for 3 hours to obtain a mixture of component B.

[0075] When used, the polyurethane electronic sponge comprises the following steps for preparation:

[0076] Add the B component mixture to the A component mixture, add 0.2 parts of the foaming agent hexane, stir for a second time at 2000 rpm for 5 minutes, pour the foamed material into the mold, and cure at 100°C for 2 hours to ensure that the material is completely cured and formed to obtain the electronic cotton polyurethane.

[0077] Comparative Example 1

[0078] The difference between this comparative example and Example 1 is that diphenylmethane diisocyanate is used instead of modified isocyanate, and the remaining steps are the same as those in Example 1.

[0079] Comparative Example 2

[0080] The difference between this comparative example and Example 2 is that hexagonal boron nitride is used instead of the intercalation material dispersion liquid, and the remaining steps are the same as those in Example 2.

[0081] Comparative Example 3

[0082] The difference between this comparative example and Example 3 is that cellulose is used instead of the intercalation material dispersion liquid, and the remaining steps are the same as those in Example 3.

[0083] Comparative Example 4

[0084] The difference between this comparative example and Example 4 is that no intercalation material dispersion liquid is added, and the remaining steps are the same as those of Example 4.

[0085] Physical property test: Referring to ASTM D792, 20g of polyurethane electronic sponges prepared in Examples 1-6 and Comparative Examples 1-4 were taken as samples for density test; referring to ASTM D412, tensile strength and elongation at break were tested on each sample. The results are shown in Table 1:

[0086] Table 1. Physical properties test results of each sample

[0087]

[0088]

[0089] Thermal stability test: Take 5 mg of sample, use thermogravimetric analyzer, set the temperature range from 50℃ to 600℃, the heating rate is 10℃ / min, record the mass loss of each sample at different temperatures, and analyze the thermal stability of the sample, including the starting decomposition temperature, the maximum decomposition rate temperature and the residual mass. The results are shown in Table 2:

[0090] Table 2. Thermal stability test results of each sample

[0091] serial number Initial decomposition temperature (℃) Maximum decomposition rate temperature (℃) Residual mass (mg) Example 1 220 390 1.8 Example 2 210 410 1.8 Example 3 220 390 1.9 Example 4 220 410 1.8 Example 5 210 400 1.9 Example 6 200 410 1.9 Comparative Example 1 150 300 0.5 Comparative Example 2 190 330 0.9 Comparative Example 3 190 340 1.0 Comparative Example 4 170 310 0.8

[0092] Aging resistance test: Before the aging test, the tensile strength and elongation at break of each sample were tested and recorded as the initial value. Each 10g sample was exposed to ultraviolet light (340nm wavelength, 0.89W / m 2 ) and the exposure time was 100h. The color change of the samples before and after exposure was measured using a colorimeter, and the ΔE value (color difference index) was recorded. After the aging test, the tensile strength and elongation at break of each sample were retested, and the retention rate of the mechanical properties was calculated, and the retention rate = (performance after aging / initial performance) × 100%. The results are shown in Table 3:

[0093] Table 3. Aging resistance test results of each sample

[0094]

[0095]

[0096] It can be seen from Table 1 that the density of the embodiments is generally higher than that of the comparative examples, and the tensile strength and elongation at break of the embodiments are better than those of the comparative examples, indicating that the materials prepared in the embodiments have good mechanical properties, which may be because the modified isocyanate provides a better cross-linking structure, while the hexagonal boron nitride and cellulose enhance the strength and toughness of the material.

[0097] It can be seen from Table 2 that the thermal stability starting decomposition temperature, maximum decomposition rate temperature and residual mass of the embodiment are significantly better than those of the comparative example, indicating that the material prepared in the embodiment has higher thermal stability, which may be because the modified isocyanate has higher thermal stability, and the hexagonal boron nitride and cellulose also act as a thermal barrier.

[0098] As shown in Table 3, the color change of the embodiment is significantly smaller than that of the comparative example, indicating that the material prepared in the embodiment is less likely to change color under ultraviolet irradiation. The mechanical property retention rate of the embodiment is also better than that of the comparative example, further proving that the material prepared in the embodiment has good aging resistance. This may be because the modified isocyanate provides a more stable cross-linked structure, while the hexagonal boron nitride and cellulose also play a role in protecting the material from ultraviolet damage.

[0099] In summary, the electronic cotton polyurethane composite material and the electronic cotton products prepared in the examples have good physical properties, thermal stability and aging resistance. Under high-intensity ultraviolet irradiation, the color change of the examples is less obvious.

[0100] In the description of the specification, the description with reference to the terms "preparation example", "embodiment", "various embodiments" and the like means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or preparation example are included in at least one embodiment or preparation example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or preparation example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or preparation examples in a suitable manner.

[0101] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A polyurethane composite material for electronic cotton, characterized in that: The invention comprises component A and component B, wherein component A comprises, by weight, 90-100 parts of modified isocyanate, 1-5 parts of silicone oil and 0.002-0.006 parts of flame retardant, and component B comprises, by weight, 120-150 parts of polyether polyol, 30-50 parts of intercalation material dispersion, 0.5-0.8 parts of diluent, 0.5-5 parts of catalyst and 0.1-3 parts of color paste.

2. The polyurethane composite material for electronic sponge according to claim 1, characterized in that: The intercalation material dispersion is prepared by the following steps: Hexagonal boron nitride and cellulose are added into ethanol, ultrasonically treated, a silane coupling agent is added, and the temperature is controlled to react to obtain an intercalation material dispersion.

3. The polyurethane composite material for electronic sponge according to claim 1, characterized in that: The modified isocyanate is prepared by the following steps: Add boron phosphide powder to diphenylmethane diisocyanate, stir at 80-90°C at a stirring speed of 300-400 rpm for 30-60 minutes, then add glutaraldehyde, and continue stirring at the same speed for 5-15 minutes to obtain modified isocyanate.

4. The polyurethane composite material for electronic sponge according to claim 2, characterized in that: The mass ratio of hexagonal boron nitride, cellulose, ethanol and silane coupling agent is (0.8-1.8): (0.5-1.5): (10-20): (0.04-0.08).

5. The polyurethane composite material for electronic sponge according to claim 2, characterized in that: The frequency of ultrasonic treatment is 20-30kHz, the power is 100-200W, the time of ultrasonic treatment is 10-30min, the reaction temperature is 60-70°C, and the reaction time is 2-4h.

6. The polyurethane composite material for electronic sponge according to claim 1, characterized in that: The catalyst includes one or more of bisdimethylaminoethyl ether, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, triethylamine, triethylenediamine, and N-methyldiethanolamine.

7. The polyurethane composite material for electronic sponge according to claim 3, characterized in that: The mass ratio of diphenylmethane diisocyanate, boron phosphide powder and glutaraldehyde is (120-150):(8-12):(1-3).

8. The polyurethane composite material for electronic sponge according to claim 1, characterized in that: The diluent includes one or more of propylene glycol methyl ether, triethylene glycol, ethylene glycol, dipropylene glycol, glycerol and water; the polyether polyol includes one or more of polypropylene glycol, polyethylene glycol and polytetramethylene glycol; and the flame retardant is aluminum hydroxide or magnesium hydroxide.

9. The preparation process of the polyurethane composite material for electronic cotton according to any one of claims 1 to 8, characterized in that: The following steps are involved: Component A: Add modified isocyanate, silicone oil and flame retardant into a mixer and stir for the first time at a stirring speed of 1000-1200 rpm for 10-20 min to obtain a mixture of component A; Component B: Add polyether polyol, intercalation material dispersion, diluent, catalyst and color paste into the mixer, stir for the second time at a speed of 2000-2500rpm for 30-60s, and keep warm at 70-80℃ for 2-3h to obtain a mixture of component B.

Citation Information

Patent Citations

  • Heat-conducting gel with low density and high flexibility and preparation method thereof

    CN115651393A

  • Hexagonal boron nitride nanosheet as well as preparation method and application thereof

    CN116395649A

  • Hard flame-retardant polyurethane foam and preparation method thereof

    CN116515070A