Preparation method of regenerated cellulose membrane
By using the combination technology of 1-ethyl-3-methylimidazole phosphate solution and water, glycerin aqueous solution and silica sol, the problem of poor solvent corrosion and light translucency in the preparation of existing regenerated cellulose films is solved, and high transparency is achieved , high strength and flexibility of regenerated cellulose film preparation, suitable for industrial production.
Patent Information
- Application Number
- CN202410991040.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing regenerated cellulose film preparation process, solvents are highly corrosive to the equipment, poor light transmittance of the finished product, and complex process, which is not conducive to industrial production.
The pulp is dissolved by 1-ethyl-3-methylimidazole phosphate solution, and the regenerated cellulose membrane is prepared by heating, filtration, water washing, plasticizing and oiling, drying, etc., using water as a solidification bath. A mixed solution of glycerol aqueous solution and silica sol is used as the plasticizing solution.
It improves the dissolution efficiency and transparency of cellulose, enhances the strength and flexibility of the film, reduces the corrosion of the equipment and production costs, and realizes the preparation of regenerated cellulose films with high transparency and high strength.
Smart Images

Figure BDA0004958883640000041 
Figure BDA0004958883640000051 
Figure BDA0004958883640000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomass resource utilization, and in particular to a method for preparing a regenerated cellulose film. Background Art
[0002] As environmental pollution becomes increasingly serious and consumers' demand for green and environmentally friendly products increases, regenerated cellulose, as a natural, renewable and environmentally friendly biomass material, has gradually attracted people's attention. Regenerated cellulose is extracted from natural plant fibers such as cotton and wood pulp. It has excellent renewability, biodegradability and biocompatibility, and is suitable for the manufacture of biomass-based materials and various environmentally friendly products. Among them, the research and application of regenerated cellulose membrane materials have developed rapidly.
[0003] Regenerated cellulose film is a new type of film material made from regenerated cellulose raw materials. It has the advantages of being eco-friendly, high in strength, high in transparency, and biodegradable. It has broad application prospects in the fields of packaging, medical supplies, etc. When regenerated cellulose film is prepared by the solvent method, there are problems such as the solvent being highly corrosive to the film-making equipment and pipelines, the finished cellulose film being turbid and having poor light transmittance, and the preparation process being complicated, which is not conducive to industrial production. Summary of the invention
[0004] In view of the problems and shortcomings in the prior art, the present invention aims to provide a method for preparing a regenerated cellulose film.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides a method for preparing a regenerated cellulose film, comprising the following steps:
[0007] (1) immersing the crushed pulp in an ionic liquid solution until the immersion is complete to obtain a mixture, wherein the ionic liquid solution is a 1-ethyl-3-methylimidazole phosphate solution;
[0008] (2) heating and dissolving the mixture, and filtering to obtain a cellulose ionic liquid solution;
[0009] (3) transporting the cellulose ionic liquid solution into a coagulation bath to prepare a film;
[0010] (4) The film is sequentially subjected to water washing, plasticizing and oiling, drying, and balanced moisture regain treatment to obtain a regenerated cellulose film.
[0011] According to the above preparation method, preferably, the ionic liquid solution in step (1) is an ionic liquid aqueous solution, and the mass fraction of 1-ethyl-3-methylimidazole phosphate in the ionic liquid solution is 55% to 80%; more preferably, the mass fraction of 1-ethyl-3-methylimidazole phosphate in the ionic liquid solution is 65% to 80%.
[0012] According to the above preparation method, preferably, in step (1), the mass ratio of pulp to ionic liquid solution is 1:(9-13.28).
[0013] According to the above preparation method, preferably, the pulp is at least one of biomass Juncao pulp, wood pulp, cotton pulp, bamboo pulp, and recycled waste cellulose. More preferably, the pulp is biomass Juncao pulp.
[0014] According to the above preparation method, preferably, in step (3), the coagulation bath is water; more preferably, the coagulation bath is desalted water; most preferably, the silicon dioxide content in the desalted water is ≤100 μg / L, and the pH of the desalted water is 6.0.
[0015] According to the above preparation method, preferably, the temperature of the coagulation bath is 10°C to 45°C; more preferably, the temperature of the coagulation bath is 30°C to 45°C.
[0016] According to the above preparation method, preferably, the solidification time is 3 to 15 seconds.
[0017] According to the above preparation method, preferably, the plasticizing liquid used in the plasticizing and oiling process in step (4) is a mixture of glycerol aqueous solution and silica sol; more preferably, the mass ratio of glycerol aqueous solution to silica sol in the plasticizing liquid is 1-3:1-7, and the mass fraction of glycerol in the glycerol aqueous solution is 6%-9.5%; the concentration of silicon dioxide in the silica sol is 10g / L-80g / L; more preferably, the concentration of silicon dioxide in the silica sol is 60g / L-80g / L.
[0018] According to the above preparation method, preferably, the pH of the plasticized liquid is 8.0-9.5; more preferably, the pH of the plasticized liquid is 8.0-9.0.
[0019] According to the above preparation method, preferably, the temperature of the plasticizing and oiling treatment is 25°C to 45°C.
[0020] According to the above preparation method, preferably, the immersion temperature in step (1) is 10°C to 110°C; more preferably, the immersion temperature is 45°C to 65°C.
[0021] The temperature for heating and dissolving in step (2) is 80°C to 150°C; more preferably, the temperature for heating and dissolving is 80°C to 150°C.
[0022] The second aspect of the present invention provides a regenerated cellulose film prepared by the preparation method described in the first aspect.
[0023] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0024] (1) The present invention uses 1-ethyl-3-methylimidazole phosphate solution as an ionic liquid solvent to dissolve the pulp. The ionic liquid solvent is transparent in color, low in viscosity, and good in stability. It can promote the rapid and efficient dissolution of cellulose, greatly improving the dissolution of cellulose. Moreover, the prepared regenerated cellulose film has high transparency (the maximum transmittance can reach 91% or more), and the breaking length of the film can reach 6490m. In addition, the ionic liquid solution is non-corrosive to equipment, and the corrosion resistance requirements of the production equipment are not high. The operation process is safe and environmentally friendly. The ionic solution can be recycled and reused through filtration, electrodialysis and evaporation.
[0025] (2) The present invention uses water as the coagulation bath. Compared with the traditional coagulation bath, it has the characteristics of low cost, non-corrosiveness, and green environmental protection. It is a leap forward in the regenerated cellulose membrane industry and plays a leading role in the development of the industry.
[0026] (3) The present invention adopts a mixed solution obtained by mixing a glycerol aqueous solution and a silica sol in a mass ratio of 1 to 3:1 to 7 as a plasticizing liquid. The plasticizing liquid can not only make the regenerated cellulose film after plasticizing and oiling treatment non-sticky and easy to roll up, but also effectively improve the flexibility and softness of the prepared regenerated cellulose film, thereby solving the problem that the existing regenerated cellulose film is brittle and easy to break.
[0027] (4) When the mixture of the mushroom grass pulp and the ionic liquid solution is heated and dissolved, the heating and dissolving temperature is controlled to be 80°C to 150°C. This temperature can not only achieve rapid dissolution of cellulose in the pulp, but also effectively avoid degradation of the cellulose polymerization degree.
[0028] (5) The regenerated cellulose film prepared by the method of the present invention has high transparency, high strength, good flexibility and good mechanical properties, which are significantly higher than the existing regenerated cellulose film preparation process; moreover, the regenerated cellulose film has good biodegradability and is environmentally friendly.
[0029] (6) The present invention preferably uses biomass Juncao pulp as raw material. Juncao has the characteristics of wide planting area, extremely rich yield and low price. Using Juncao to prepare regenerated cellulose film can not only realize the resource utilization of Juncao, but also effectively reduce the production cost of regenerated cellulose film, and alleviate the problem of insufficient raw materials for existing regenerated cellulose film; moreover, through the high-value resource utilization of biomass Juncao, "replacing wood with grass" can reduce the felling of trees and further protect the ecological environment. DETAILED DESCRIPTION
[0030] The following examples are only for further explanation of the present invention. It should be noted that all technical and scientific terms used in the present invention have the same meanings as in the technical field to which the present invention belongs unless otherwise specified. The experimental methods in the following examples without specifying specific conditions are all based on conventional techniques in the technical field, or according to the conditions recommended by the manufacturer; the reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.
[0031] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0032] Example 1: Experiment on the types of coagulation baths
[0033] In order to study the effect of the type of coagulation bath on the preparation of regenerated cellulose film, the present invention carried out Example 1-1, Comparative Example 1-1 to Comparative Example 1-2. The specific contents of Example 1-1, Comparative Example 1-1 to Comparative Example 1-2 are as follows:
[0034] Example 1-1:
[0035] A method for preparing a regenerated cellulose film, characterized in that the specific steps are as follows:
[0036] (1) The biomass grass pulp is pulverized, and the pulverized biomass grass pulp is immersed in an ionic liquid solution at 55° C. for 10 minutes to obtain a mixture; wherein the mass ratio of the biomass grass pulp to the ionic liquid solution is 1:9, and the ionic liquid solution is an aqueous solution of 1-ethyl-3-methylimidazole phosphate; and the mass fraction of 1-ethyl-3-methylimidazole phosphate in the ionic liquid solution is 74%.
[0037] (2) The mixed material obtained in step (1) is heated and dissolved, filtered, and degassed to obtain a cellulose ionic liquid solution; wherein the heating and dissolving temperature is 85° C. to 90° C., and the heating and dissolving time is 60 min.
[0038] (3) using a melt pump to spray the cellulose ionic liquid solution obtained in step (2) into a coagulation bath through a melt pump nozzle, coagulating for 3 seconds to prepare a film; wherein the coagulation bath is desalted water, the silica content in the desalted water is ≤100 μg / L, and the pH of the desalted water is 8.0-9.5; and the temperature of the coagulation bath is 25°C.
[0039] (4) sending the film obtained in step (3) into a water washing tank for water washing, wherein the water washing temperature of the water washing tank is set to 25° C., 35° C., and 30° C., respectively; immersing the washed film in a plasticizing liquid with a pH of 6 at 25° C., and plasticizing and oiling for 50 seconds; wherein the plasticizing liquid is a mixture of a glycerol aqueous solution and a silica sol in a mass ratio of 1:1, wherein the mass fraction of glycerol in the glycerol aqueous solution is 8%, and the concentration of silicon dioxide in the silica sol is 70 g / L.
[0040] (5) The film treated in step (4) is dried at 45° C. for 60 seconds, and then transferred to a balanced moisture-recovery room for balanced moisture-recovery at a temperature of 45° C. and a relative humidity of 50% RH, and the moisture content of the film is controlled at about 5%, thereby obtaining a regenerated cellulose film with a thickness of 0.05 mm.
[0041] Comparative Example 1-1:
[0042] The contents of Comparative Example 3-1 are substantially the same as those of Example 1-1, except that in step (3), the coagulation bath is ethanol.
[0043] Comparative Example 1-2:
[0044] The content of Comparative Example 3-2 is substantially the same as that of Example 1-1, except that in step (3), the coagulation bath is propylene glycol.
[0045] In order to verify the influence of the type of ionic liquid on the performance of the prepared regenerated cellulose membrane, the performance of the regenerated cellulose membrane prepared in Example 1-1 and Comparative Examples 1-1 to 1-2 was tested. The test results are shown in Table 1 below.
[0046] Table 1 Effect of coagulation bath type on the properties of regenerated cellulose membrane
[0047]
[0048] It can be seen from Table 1 that when water, ethanol or propylene glycol is used as the coagulation bath, the transmittance and elongation of the prepared regenerated cellulose film are less affected. However, when water is used as the coagulation bath, the prepared regenerated cellulose film has a long breaking length and a good tear strength index. Therefore, water is preferably used as the coagulation bath.
[0049] Example 2: Experiment on the types of plasticizing liquid
[0050] In order to study the effect of the type of plasticizer on the preparation of regenerated cellulose film, the present invention conducted comparative examples 2-1 to 2-2. The specific contents of comparative examples 2-1 to 2-2 are as follows:
[0051] Comparative Example 2-1:
[0052] The content of Comparative Example 2-1 is substantially the same as that of Example 1-1, except that in step (4), the plasticizing liquid is a glycerol aqueous solution, and the mass fraction of glycerol in the glycerol aqueous solution is the same as that of Example 1-1.
[0053] Comparative Example 2-2:
[0054] The content of Comparative Example 2-2 is substantially the same as that of Example 1-1, except that in step (3), the plasticizing liquid is silica sol, and the concentration of silicon dioxide in the silica sol is the same as that of Example 1-1.
[0055] In order to verify the influence of the type of ionic liquid on the performance of the prepared regenerated cellulose membrane, the performance of the regenerated cellulose membrane prepared in Example 1-1 and Comparative Example 2-1 to Comparative Example 2-2 was tested. The test results are shown in Table 2 below.
[0056] Table 2 Effect of plasticizer type on the properties of regenerated cellulose film
[0057]
[0058] It can be seen from Table 2 that when a mixture of glycerol aqueous solution and silica sol is used as the plasticizing liquid, the breaking length, tear strength, transmittance and elongation of the prepared regenerated cellulose film are significantly better than those of glycerol aqueous solution and silica sol. Therefore, the plasticizing liquid is preferably a mixture of glycerol aqueous solution and silica sol.
[0059] Example 3: Discussion on the mass ratio of glycerol aqueous solution to silica sol in plasticizing liquid
[0060] In order to study the effect of the mass ratio of glycerol aqueous solution to silica sol in the plasticizing liquid on the preparation of regenerated cellulose film, the present invention carried out Examples 3-1 to 3-3. The specific contents of Examples 3-1 to 3-3 are as follows:
[0061] Example 3-1:
[0062] The content of Example 3-1 is basically the same as that of Example 1-1, except that in step (4), the mass ratio of the glycerol aqueous solution to the silica sol in the plasticizing liquid is 3:2.
[0063] Example 3-2:
[0064] The content of Example 3-2 is basically the same as that of Example 1-1, except that in step (4), the mass ratio of the glycerol aqueous solution to the silica sol in the plasticizing liquid is 2:3.
[0065] Example 3-3:
[0066] The content of Example 3-3 is basically the same as that of Example 1-1, except that in step (4), the mass ratio of the glycerol aqueous solution to the silica sol in the plasticizing liquid is 3:7.
[0067] In order to verify the effect of the mass ratio of glycerol aqueous solution to silica sol in the plasticizing liquid on the performance of the prepared regenerated cellulose film, the performance of the regenerated cellulose films prepared in Example 1-1 and Example 3-1 to Example 3-3 were tested, and the test results are shown in Table 3 below.
[0068] Table 3 Effect of the mass ratio of glycerol aqueous solution to silica sol on the properties of regenerated cellulose membrane
[0069]
[0070] It can be seen from Table 3 that when the mass ratio of glycerol aqueous solution to silica sol is adjusted from 3:2, 1:1, 2:3 to 3:7, the improvement effect of various performance indicators of the obtained regenerated cellulose membrane is not obvious. The regenerated cellulose membrane prepared with a glycerol: silica sol ratio of 1:1 has the best performance. Therefore, the mass ratio of glycerol aqueous solution to silica sol is preferably 1:1.
[0071] Example 4: Experimental study on the types of ionic liquids
[0072] In order to study the effect of ionic liquid types on the preparation of regenerated cellulose membranes, the present invention conducted comparative example 4-1. The specific contents are as follows:
[0073] Comparative Example 4-1:
[0074] The content of Comparative Example 4-1 is substantially the same as that of Example 1-1, except that in step (1), the ionic liquid solution is an aqueous solution of 1-allyl-3-methylimidazolium chloride.
[0075] In order to verify the influence of the type of ionic liquid on the performance of the prepared regenerated cellulose membrane, the performance of the regenerated cellulose membrane prepared in Example 1-1 and Comparative Example 4-1 was tested, and the test results are shown in Table 4 below.
[0076] Table 4 Effect of ionic liquid types on the properties of regenerated cellulose membranes
[0077]
[0078]
[0079] It can be seen from Table 4 that compared with 1-allyl-3-methylimidazolium chloride, when the ionic liquid solution is 1-ethyl-3-methylimidazolium phosphate aqueous solution, the prepared regenerated cellulose film has good performance indicators of breaking length, tear strength, transmittance and elongation.
[0080] Example 5: Experimental study on the dosage of ionic liquid
[0081] In order to study the effect of the amount of ionic liquid on the preparation of regenerated cellulose membrane, the present invention carried out Examples 5-1 to 5-4. The specific contents of Examples 5-1 to 5-4 are as follows:
[0082] Example 5-1:
[0083] The content of Example 5-1 is basically the same as that of Example 1-1, except that in step (1), the mass ratio of the pulp to the ionic liquid solution is 1:10.11.
[0084] Example 5-2:
[0085] The content of Example 5-2 is basically the same as that of Example 1-1, except that in step (1), the mass ratio of the pulp to the ionic liquid solution is 1:11.5.
[0086] Example 5-3:
[0087] The content of Example 5-3 is basically the same as that of Example 1-1, except that in step (1), the mass ratio of the pulp to the ionic liquid solution is 1:12.33.
[0088] Example 5-4:
[0089] The content of Example 5-4 is basically the same as that of Example 1-1, except that in step (1), the mass ratio of the pulp to the ionic liquid solution is 1:13.28.
[0090] In order to verify the effect of the amount of ionic liquid on the performance of the prepared regenerated cellulose membrane, the performance of the regenerated cellulose membranes prepared in Examples 5-1 to 5-4 was tested. The test results are shown in Table 5 below.
[0091] Table 5 Effect of ionic liquid dosage on the properties of regenerated cellulose membrane
[0092]
[0093]
[0094] It can be seen from Table 5 that the smaller the pulp mass ratio, the smaller the breaking length, the smaller the tear strength, the better the transmittance, and the slightly decreased elongation. Among them, the regenerated cellulose film prepared with a mass ratio of pulp to ionic liquid solution of 1:11.5 has better comprehensive performance in breaking length, tear strength, transmittance and elongation.
[0095] The above embodiments are specific implementation methods of the present invention, but the implementation methods of the present invention are not limited to the above embodiments. Any other combination, change, modification, substitution and simplification that does not exceed the design concept of the present invention shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a regenerated cellulose film, characterized in that: The following steps are involved: (1) impregnating the pulverized pulp in an ionic liquid solution until the impregnation is complete to obtain a mixture, wherein the ionic liquid solution is a 1-ethyl-3-methylimidazole phosphate solution; (2) heating and dissolving the mixture, and filtering to obtain a cellulose ionic liquid solution; (3) transporting the cellulose ionic liquid solution into a coagulation bath to prepare a film; (4) The film is sequentially subjected to water washing, plasticizing and oiling, drying, and balanced moisture regain treatment to obtain a regenerated cellulose film.
2. The preparation method according to claim 1, characterized in that: The mass fraction of 1-ethyl-3-methylimidazole phosphate in the ionic liquid solution in step (1) is 55% to 80%.
3. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of pulp to ionic liquid solution is 1:(9-13.28); the pulp is at least one of biomass grass pulp, wood pulp, cotton pulp, bamboo pulp, and recovered cellulose.
4. The preparation method according to any one of claims 1 to 3, characterized in that: In step (3), the coagulation bath is water.
5. The preparation method according to claim 4, characterized in that: The coagulation bath is desalted water, the silicon dioxide content in the desalted water is ≤100 μg / L, and the pH of the desalted water is 8.0-9.
5.
6. The preparation method according to claim 4, characterized in that: The temperature of the coagulation bath is 10° C. to 45° C., and the coagulation time is 3 to 15 seconds.
7. The preparation method according to claim 6, characterized in that: In step (4), the plasticizing liquid used in the plasticizing and oiling process is a mixture of glycerol aqueous solution and silica sol, and the mass ratio of glycerol aqueous solution to silica sol in the plasticizing liquid is 1-3:1-7.
8. The preparation method according to claim 7, characterized in that: The mass fraction of glycerol in the glycerol aqueous solution is 6% to 9.5%, the concentration of silicon dioxide in the silica sol is 10g / L to 80g / L; the pH of the plasticizing liquid is 8.0 to 9.5; and the temperature of the plasticizing oiling treatment is 25°C to 45°C.
9. The preparation method according to claim 8, characterized in that: The immersion temperature in step (1) is 10°C to 110°C; the heating and dissolving temperature in step (2) is 80°C to 150°C.
10. A regenerated cellulose film prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Plasticizing liquid for preparing ionic liquid regenerated cellulose membrane and detection method of silicon content of plasticizing liquid
CN122591463A