Color paste capable of transferring surface of product as well as preparation method and application of color paste

By using methyl oleate and maleate combination materials in pultruded fiberglass, the color paste is migrated to the product surface, which solves the problem of traditional color paste affecting the internal quality of the profile and achieves high-quality and uniform colored fiberglass. surface.

CN118930971APending Publication Date: 2024-11-12NANJING DEJIA GLASS FIBRE REINFORCED PLASTIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975765.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The use of color paste in traditional pultruded fiberglass composite materials is large and affects the internal quality of the profile, resulting in uneven color and floating color and other problems.

Method used

Using a combination of methyl oleate, maleate, toner, dispersant and anti-flocculant, the color paste is migrated to the product surface during the pultrusion process to form a uniform color and cure, reducing the impact on internal quality. .

Benefits of technology

The uniform migration and curing of color paste is achieved, the amount of color paste is reduced, the product quality and color uniformity is improved, the internal quality influence is reduced, and the weather resistance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930971A_ABST
    Figure CN118930971A_ABST
Patent Text Reader

Abstract

The invention discloses color paste on the surface of a transferable product and a preparation method and application of the color paste, the color paste on the surface of the transferable product comprises the following raw material components: 15-20% of methyl oleate, 38-43% of toner, 30-35% of maleate, 0.5-1.5% of silicon dioxide, 3-5% of a dispersing agent and 3-5% of a deflocculating agent, the sum of the mass percentage of all the raw material components is 100%, and the percentage is mass percentage. According to the color paste capable of migrating the surface of the product, the color paste can migrate to the surface of the product in the pultrusion glass fiber reinforced plastic forming process, the tinting strength is high, the color is uniform and attractive, and flocculation, color fading and floating are avoided; the use amount of color paste is reduced, and the total cost is reduced; meanwhile, the influence of color paste on the internal quality of the profile is reduced, and the product quality is improved. The preparation is simple and convenient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a color paste capable of migrating to the surface of a product, a preparation method and application thereof, and belongs to the technical field of color pastes for pultruded glass fiber reinforced plastic composite materials. Background Art

[0002] FRP is a reinforced plastic that uses glass fiber or its products as reinforcement materials, called glass fiber reinforced plastic. Due to the different types of resins used, it can be divided into polyester FRP, epoxy FRP, phenolic FRP, etc.

[0003] FRP has the advantages of being light and hard, non-conductive, stable in performance, high in mechanical strength, and corrosion-resistant. It has been widely used in various fields such as construction, automobiles, energy, and electronics. On the basis of meeting the strength requirements, it not only reduces weight but also greatly reduces economic costs.

[0004] The pultrusion process is to form and solidify continuous glass fiber bundles, tapes or cloths impregnated with resin glue containing color paste through an extrusion die under the action of traction, and continuously produce pultruded FRP profiles of unlimited length. It is widely used in electrical / appliances, corrosion-resistant solutions, construction, transportation, military and consumer products.

[0005] The color paste is added to distinguish the color. The color paste of traditional pultruded FRP composite materials is added to the FRP pultruded profile and evenly dispersed in the product. This not only requires a large amount of color paste, but also affects the internal quality of the profile. Summary of the invention

[0006] The present invention provides a color paste capable of migrating to the surface of a product, a preparation method thereof and an application thereof. The color paste capable of migrating to the surface of a product can migrate to the surface of the product during the process of pultruding glass fiber reinforced plastics, and the color is uniform, without flocculation, fading or floating color. The amount of the color paste can be reduced, the influence of the color paste on the internal quality of the profile can be reduced, and the product quality can be improved.

[0007] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:

[0008] A color paste capable of migrating to the surface of a product, the raw material components of which include: 15-20% methyl oleate, 38-43% toner, 30-35% maleate, 0.5-1.5% silicon dioxide, 3-5% dispersant, 3-5% deflocculant, the mass sum of the raw material components being 100%, and % being the mass percentage.

[0009] The color paste of the invention will migrate to the surface of the product during the process of pultruded glass fiber reinforced plastics forming, forming a high-quality surface with uniform hue, no flocculation, no fading, and no floating color.

[0010] The inventors believe that the principle by which the color paste of the present application can migrate to the surface of the product is that methyl oleate is incompatible with the unsaturated resin used to prepare the FRP. When the unsaturated resin with the color paste is mixed with the glass fiber, the maleate contains double bonds and is compatible and reactive with the unsaturated resin. During the pultrusion molding process in the heated mold cavity, the unsaturated resin begins to solidify. Due to its incompatibility, methyl oleate becomes a release agent between the mold cavity and the FRP profile. The color paste migrates to the surface of the FRP profile and solidifies on the surface, thereby greatly improving the weather resistance, making the color uniform and the hiding power high.

[0011] % in this application are all mass percentages unless otherwise specified.

[0012] In order to further improve the product quality of pultruded fiberglass, the above-mentioned maleate is preferably at least one of dibutyl maleate (dibutyl maleate), dimethyl maleate, diethyl maleate, diisopropyl maleate or diisooctyl maleate; further preferably, the maleate is dibutyl maleate or dimethyl maleate; more preferably, the maleate is dibutyl maleate.

[0013] When preparing black articles, the preferred black toner is REGAL 660R.

[0014] In order to further improve the coloring effect of pultruded FRP, the silica is fumed silica A200.

[0015] In order to further improve the uniformity of the material and the coloring effect of the pultruded FRP, the dispersant is dispersant BYK-W940.

[0016] In order to avoid flocculation and ensure product quality, the deflocculant is a solution of a mixture of an unsaturated polycarboxylic acid polymer and a polysiloxane copolymer, and more preferably the deflocculant NEO-7904S.

[0017] The method for preparing the color paste capable of migrating to the surface of the product comprises the following steps:

[0018] 1) Soak the toner in methyl oleate for 18 to 24 hours, then stir at 800 to 1000 rpm for 20 to 30 minutes until the toner surface is basically soaked;

[0019] 2) adding dibutyl maleate to the material obtained in step 1), stirring at 400-600 rpm for 10-20 minutes, adding silicon dioxide, stirring at high speed of 1300-1500 rpm for 10-15 minutes;

[0020] 3) Add the dispersant and the deflocculant to the material obtained in step 2), stir at 400-600 rpm for 8-12 minutes, grind with a sand mill to a fineness of less than 20 microns, and package.

[0021] It is carried out in a stainless steel barrel equipped with a high-speed disperser.

[0022] The color paste capable of migrating to the surface of a product can be used for the preparation of a glass fiber reinforced plastic pultruded composite material, and the color paste can migrate to the surface of the product during molding.

[0023] The fillers, dispersants and deflocculants of the present application may also be selected from products other than fumed silica, BYK-W940 and NEO-7904S. However, the experiment found that after silica, BYK-W940 and NEO-7904S were compounded with methyl oleate, color powder and maleate, the quality of the FRP pultruded composite material was significantly better.

[0024] In order to better ensure the performance of the obtained profile, the matrix resin used in the above-mentioned FRP pultruded composite material is an unsaturated polyester resin. 61-972; The amount of the color paste that can migrate to the surface of the product is 0.3-0.5% of the mass of the unsaturated polyester resin.

[0025] The technologies not mentioned in the present invention are all referred to the prior art.

[0026] The color paste of the invention can migrate to the surface of the product. During the process of pultruding FRP, the color paste will migrate to the surface of the product, with strong coloring power, uniform color, beautiful appearance, no flocculation, no fading, no floating color, and reduced amount of color paste, and reduced overall cost; at the same time, the influence of the color paste on the internal quality of the profile is reduced, and the product quality is improved. The preparation is simple and convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The appearance diagrams of the glass fiber reinforced plastic pultruded composite materials prepared by using the color pastes in Example 1 and Comparative Example 1 respectively;

[0028] Figure 2 is a cross-sectional view of a glass fiber reinforced plastic pultruded composite material prepared using the color paste in Example 1;

[0029] Figure 3 It is a cross-sectional view of a glass fiber reinforced plastic pultruded composite material prepared by using the color paste in Comparative Example 1; DETAILED DESCRIPTION

[0030] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0031] Color powder is 660R Pigment Black, brand: Cabot. Silica is fumed silica A200, brand: Degussa, model: AEROSIL 200. Dispersant is dispersant BYK-W940, brand: BYK, model: BYK-W 940. Deflocculant is deflocculant NEO-7904S, Wuxi Liou Chemical Materials Co., Ltd.

[0032] Unsaturated resin P50, model: P50 resin, originated from Dingyuan Hongyuan New Materials Co., Ltd.

[0033] Unsaturated polyester resin 61-972, from AOC China Jinling Aliancy Resin Co., Ltd.

[0034] Example 1

[0035] The invention discloses a color paste capable of migrating to the surface of a product. The raw materials of the color paste consist of the following components: 18 wt% of methyl oleate, 40 wt% of toner, 33 wt% of dibutyl maleate, 1 wt% of silicon dioxide, 4 wt% of a dispersant and 4 wt% of an anti-flocculant.

[0036] The method for preparing the color paste capable of migrating to the surface of the product comprises the following steps:

[0037] 1) Soak the toner in methyl oleate in a stainless steel barrel for 24 hours, then stir at 900 rpm for 30 minutes until the toner surface is basically soaked;

[0038] 2) adding dibutyl maleate to the material obtained in step 1), stirring at 500 rpm for 20 minutes, adding silicon dioxide, stirring at a high speed of 1400 rpm for 15 minutes;

[0039] 3) Add the dispersant and deflocculant to the material obtained in step 2), stir at 500 rpm for 10 minutes, grind with a sand mill to a fineness of less than 20 microns, and package. The minimum film thickness method test shows that the hiding power is 9μm and the adhesion is level 0. Temperature resistance (250℃, 2h): no discoloration.

[0040] Example 2

[0041] A color paste capable of migrating to the surface of a product, wherein the raw materials are composed of the following components: 18wt% methyl oleate, 40wt% toner, 33wt% dimethyl maleate, 1wt% silicon dioxide, 4wt% dispersant and 4wt% deflocculant. The preparation is based on Example 1, and the only difference from Example 1 is that dibutyl maleate is replaced by dimethyl maleate. The hiding power is 20μm.

[0042] The color pastes obtained in Example 1 and Example 2 do not form a skin, solidify, or precipitate during storage, and the color powder does not agglomerate, and the stability at room temperature is more than 24 months.

[0043] Comparative Example 1

[0044] A color paste, the raw materials of which are composed of the following components: 68wt% of unsaturated resin P50, 20wt% of color powder, 2wt% of dispersant and 10wt% of filler, with a covering power of 76μm.

[0045] Comparative Example 2

[0046] The invention discloses a color paste capable of migrating to the surface of a product. The raw materials of the color paste consist of the following components: 25 wt% of methyl oleate, 40 wt% of toner, 26 wt% of dibutyl maleate, 1 wt% of silicon dioxide, 4 wt% of a dispersant and 4 wt% of an antiflocculating agent.

[0047] Comparative Example 3

[0048] The invention discloses a color paste capable of migrating to the surface of a product. The raw materials of the color paste consist of the following components: 10 wt% of methyl oleate, 40 wt% of toner, 41 wt% of dibutyl maleate, 1 wt% of silicon dioxide, 4 wt% of a dispersant and 4 wt% of an antiflocculating agent.

[0049] Application Examples

[0050] The color pastes of the above examples were used to prepare glass fiber reinforced plastic pultruded composite materials.

[0051] The FRP pultruded composite material includes a matrix material and a reinforcement material, and the volume of the reinforcement material accounts for 55% of the FRP pultruded composite material.

[0052] The composition of the base material includes: 0.1-2 parts of color paste, unsaturated polyester resin 61-972 100 parts, tert-butyl perbenzoate 1 part, release agent 0.1 to 1.1 parts.

[0053] The reinforcing material is composed of alkali-free glass fiber stitched mat, alkali-free glass fiber biaxial fabric and alkali-free glass fiber yarn in a volume ratio of 1:1:1, wherein the surface density of the alkali-free glass fiber stitched mat is 300g / m 2 ; The surface density of the alkali-free glass fiber biaxial fabric is 600g / m 2 ; The linear density of the alkali-free glass fiber yarn is 9600tex and the moisture content is 0.03%.

[0054] Preparation method of FRP pultruded composite material:

[0055] 1) Put the weighed raw material components into the resin barrel, stir them with a high-speed stirrer at 1000r / min for 15 minutes to obtain a mixed glue solution;

[0056] 2) Introduce the mixed glue into the resin glue tank to fully impregnate the reinforcement material;

[0057] 3) starting the pultrusion machine, pultruding and curing the reinforcing material impregnated with the mixed adhesive to obtain a FRP pultruded profile, wherein the pultrusion line speed is 0.7 m / min, the curing temperature is 150° C., and the curing time is 40 s.

[0058] The influence of different amounts of color paste was investigated: a FRP pultruded profile with a width of 8 cm and a thickness of 0.3 cm was prepared, and the color paste in the base material was gradually increased from 0.1 parts. When 0.3 parts of the color paste of Example 1 was used, the black color could evenly cover the profile surface; while 2 parts of the color paste of Comparative Example 1 were required to obtain a black profile. Figure 1 As shown, the appearance of the profile obtained by using 0.3 parts of the color paste of Example 1 (a) and 2 parts of the color paste of Comparative Example 1 (b) is shown. Figure 1 It can be seen that the black color of the profile obtained by using 0.3 parts of the color paste in Example 1 is deeper and more uniform. The reason is that the color paste in Example 1 migrates to the surface of the fiberglass profile and solidifies evenly on the surface. This not only greatly reduces the amount of color paste used, but also makes it more uniform and beautiful. Figure 2 This is a cross-sectional view of the FRP pultruded composite material prepared using the color paste in Example 1. It can be seen intuitively from this figure that the color paste migrates and is evenly solidified on the surface of the FRP profile. Figure 3 This is a cross-sectional view of the FRP pultruded composite material produced using the color paste in Comparative Example 1. It can be seen intuitively from this figure that the traditional color paste is dispersed throughout the product.

[0059] Investigate the dosage of release agent: In the base material, the dosage of the color paste of Example 1, Example 2, Comparative Example 2 and Comparative Example 3 is 0.3 parts respectively, the dosage of the color paste of Comparative Example 1 is 2 parts, and the release agent (stearic acid) is increased from 0.1. The color paste of Example 1, Example 2 and Comparative Example 2 is 0.2 parts, which can achieve demoulding; the color paste of Comparative Example 3 is 0.6 parts, which can achieve demoulding; the color paste of Comparative Example 1 is 1.1 parts, which can achieve demoulding. The inventor believes that one of the main reasons is that methyl oleate is incompatible, which promotes the separation of the mold cavity and the glass fiber reinforced plastic profile.

[0060] The mechanical properties of the FRP pultruded profiles were investigated: in the base material, the amounts of the color pastes used in Example 1, Example 2, Comparative Example 2 and Comparative Example 3 were 0.3 parts respectively, and the amount of the color paste used in Comparative Example 1 was 2 parts; the amount of the release agent used in Example 1, Example 2 and Comparative Example 2 was 0.2 parts, the amount of the release agent used in Comparative Example 3 was 0.6 parts, and the amount of the release agent used in Comparative Example 1 was 1.1 parts; the mechanical properties were tested with reference to GB / T 1447-2005, and the results were as follows:

[0061] The effects of each example are compared as follows:

[0062] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength MPa 632 556 496 531 633 Bending strength MPa 655 538 473 508 653

[0063] As can be seen from the above table, the mechanical properties of Example 1 and Comparative Example 3 are the best, but considering that Comparative Example 3 will significantly increase the amount of release agent compared to Comparative Example 1, the color paste of Example 1 is the best after comprehensive consideration. The mechanical properties of Example 1 are significantly better than those of Comparative Example 1. The inventor believes that, on the one hand, the color paste of Example 1 migrates to the surface in a concentrated manner, reducing the impact of the color paste on the internal structure. On the other hand, the maleic acid ester in the color paste reacts with the unsaturated polyester resin, further enhancing the obvious improvement of the mechanical properties. The effect of Comparative Example 2 is worse. The inventor believes that one of the main reasons is that the amount of maleic acid ester in the color paste is reduced.

Claims

1. A color paste that can migrate to the surface of a product, Features: The raw material components include: 15-20% methyl oleate, 38-43% toner, 30-35% maleate, 0.5-1.5% silicon dioxide, 3-5% dispersant, 3-5% deflocculant, the mass sum of each raw material component is 100%, and % is mass percentage.

2. The color paste capable of migrating the surface of an article as claimed in claim 1, Features: The maleate is at least one of dibutyl maleate, dimethyl maleate, diethyl maleate, diisopropyl maleate or diisooctyl maleate.

3. The color paste capable of migrating the surface of the product as claimed in claim 2, Features: The maleate is dibutyl maleate or dimethyl maleate.

4. The color paste capable of migrating the surface of the product as claimed in claim 3, Features: The maleate ester is dibutyl maleate.

5. The color paste capable of migrating the surface of an article as claimed in any one of claims 1 to 4, Features: The silicon dioxide is fumed silicon dioxide A200; and the dispersant is dispersant BYK-W940.

6. The color paste capable of migrating the surface of an article as claimed in any one of claims 1 to 4, Features: The deflocculant is a solution of a mixture of an unsaturated polycarboxylic acid polymer and a polysiloxane copolymer.

7. The color paste capable of migrating the surface of an article as claimed in claim 6, Features: The anti-flocculant is anti-flocculant NEO-7904S.

8. A method for preparing a color paste capable of migrating onto the surface of a product according to any one of claims 1 to 7, Features: The steps include: 1) Soaking the toner in methyl oleate for 18 to 24 hours, and then stirring at a speed of 800 to 1000 rpm for 20 to 30 minutes; 2) adding dibutyl maleate to the material obtained in step 1), stirring at 400-600 rpm for 10-20 minutes, adding silicon dioxide, stirring at high speed of 1300-1500 rpm for 10-15 minutes; 3) Add the dispersant and the deflocculant to the material obtained in step 2), stir at 400-600 rpm for 8-12 minutes, grind with a sand mill to a fineness of less than 20 microns, and package.

9. Use of the color paste of any one of claims 1 to 7 that can be transferred to the surface of an article, Features: Used in the preparation of FRP pultruded composite materials, and the migration of color paste to the surface of products during molding.

10. The use according to claim 9, Features: The matrix resin used in FRP pultruded composite materials is unsaturated polyester resin 61-972; The amount of the color paste that can migrate to the surface of the product is 0.3-0.5% of the mass of the unsaturated polyester resin.